Hi friends,

 

We have a big pipe line job in water segment.

We are planning to implement FCAW or GMAW technique to expedite the welding activity…

Please suggest me that which technique is most favorable for IS2062 material (equivalent to Pno 1) at site for 5G or 6G position…..

Your detail explanation will be more helpful on selecting the process….

Also in terms of cost – which will be economical for the project ….

 

Thanks & Regards,

Lakshman Kumar B,

Project Manager.

 

Navayuga Engineering Company LTD

Corp Off: Plot no 379, Road No 10,

Jubileehills, Hyderabad.500033 India.

Tel -  +91 -40-2333 9990/91/92 – Ext 398

Fax: +91-40-2333 7789

Mob - +91 9440031459.

Email –lakshma...@navayuga.com

http://www.necltd.com/

cid:image001.jpg@01D1CBAD.24B27170

 

image001.jpg

Kannayeram Gnanapandithan

ungelesen,
26.10.2016, 02:19:1726.10.16
an materials-welding
it is better to go with FCAW because consumable is suitable for all position welding

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Wed, Oct 26, 2016 at 9:56 AM, Lakshman Kumar. B <lakshma...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (lakshma...@gmail.com) Add cleanup rule | More info
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/003601d22f41%241a710580%244f531080%24%40gmail.com.
For more options, visit https://groups.google.com/d/optout.


dilintas

ungelesen,
26.10.2016, 02:38:1726.10.16
an material...@googlegroups.com
GMAW is prone to lack of fusion



Sent from my Samsung Galaxy smartphone.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4ePw3gXNgxXZntjZ_wkY5Z4yiAvZvUOHb4YQbRSBnktNWQ%40mail.gmail.com.

Neilashkumar

ungelesen,
26.10.2016, 07:03:0826.10.16
an material...@googlegroups.com
Dear Lakshman,

Can you please tell us the size of the pipe and thickness in order to choose the suitable weld process? It's like need to be automated in terms of orbital type.

I will be able to give more input on hearing the above queries .

P.NEILASHKUMAR 
Sent from my iPad
MOB : 966 551094590
             +91 9952110791

<image001.jpg>

 

aslab khan

ungelesen,
26.10.2016, 07:03:1426.10.16
an material...@googlegroups.com
Flux-cored wire is considered to have some advantages for outdoor welding on-site, as the shielding gas plume is less likely to be blown away in a wind than shield gas from a conventional nozzle. A slight drawback is that, like SMAW (stick) welding, there may be some flux deposited over the weld bead, requiring more of a cleaning process between passes.

consider FCAW better in your case.




Thanks & Regards,
Aslab Ahmad Khan
QA/QC Inspector
Samsung Engineering Co.Ltd.Takreer CBDC PRJ(abudhabi)
Hello:+971-568436534(abudhabi),
Mail @ asla...@gmail.com
 

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

Lakshman Kumar. B

ungelesen,
26.10.2016, 22:35:3826.10.16
an material...@googlegroups.com

Hi Mr. Neilash Kumar,

 

It is 120 Inch (3000Mm Dia) with 20 mm thick for a water transmission project.

 

Thanks & Regards,

Lakshman Kumar B,

prem_nautiyal26

ungelesen,
26.10.2016, 22:36:4826.10.16
an material...@googlegroups.com
It will be better to go for FCAW in order to have much better quality Welds and productivity.
Also E71T1 can be welded in any position with radiographic quality.

Also how come you will be getting IS 2062 material in pipe form??

Your pipes may be A 106 GrB or IS 1239 or API 5L.


Regards

Prem Nautiyal 
Cell 9769316004




Sent from my Samsung Galaxy smartphone.

-------- Original message --------
From: "Lakshman Kumar. B" <lakshma...@gmail.com>
Date: 26/10/2016 09:56 (GMT+05:30)
Subject: [MW:25601] Comparison for FCAW & GMAW

Hi friends,

 

We have a big pipe line job in water segment.

We are planning to implement FCAW or GMAW technique to expedite the welding activity…

Please suggest me that which technique is most favorable for IS2062 material (equivalent to Pno 1) at site for 5G or 6G position…..

Your detail explanation will be more helpful on selecting the process….

Also in terms of cost – which will be economical for the project ….

 

Thanks & Regards,

Lakshman Kumar B,

Project Manager.

 

Navayuga Engineering Company LTD

Corp Off: Plot no 379, Road No 10,

Jubileehills, Hyderabad.500033 India.

Tel -  +91 -40-2333 9990/91/92 – Ext 398

Fax: +91-40-2333 7789

Mob - +91 9440031459.

Email –lakshma...@navayuga.com

http://www.necltd.com/

cid:image001.jpg@01D1CBAD.24B27170

 

Alan Denney

ungelesen,
26.10.2016, 22:36:4826.10.16
an material...@googlegroups.com


Sent: 26 October 2016 07:23
To: material...@googlegroups.com

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/003601d22f41%241a710580%244f531080%24%40gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4ePw3gXNgxXZntjZ_wkY5Z4yiAvZvUOHb4YQbRSBnktNWQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.


For more options, visit https://groups.google.com/d/optout.


This email has been scanned by BullGuard antivirus protection.
For more info visit www.bullguard.com
image002.jpg

pgoswami

ungelesen,
26.10.2016, 23:43:3926.10.16
an material...@googlegroups.com

Hi Lakhsman,

 

Both the processes are popular choices for pipeline welding. Mechanization  is the key. In general controlled surface transfer process e.g. STT or RMD are very conveniently used for long pipeline welding projects to cut down the production time and defect rates.

 

The attached documents provide some insights to such projects. Use the info at your discretion.

 

Thanks.

 

 

 

Pradip Goswami, P.Eng,IWE
 Welding & Metallurgical Engineering Specialist ,

ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 


To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/008401d22fb6%245faad430%241f007c90%24%40gmail.com.
Mechanized-Pipeline-Welding-Magnatec.pdf

Neilashkumar

ungelesen,
27.10.2016, 02:16:1727.10.16
an material...@googlegroups.com
Dear Lakshman,

Good morning, as told by Pradip sir it's has to be root weld by GMAW-STT, followed by  SAW -Machine Welding column and boom with roller bed both in site or shop.
Since 3meter OD little bit difficult with Mechanisation process, and I have practical experience with Magna tech and lone star machine up to 48 inch only.
I don't see any external band for 3meter OD.
Even in machine welding in order to increase productivity you can choose Twin wire SAW process.
Further any clarification let me know to clarify.

P.NEILASHKUMAR 
Sent from my iPad
MOB : 966 551094590
             +91 9952110791

For more options, visit https://groups.google.com/d/optout.
<Mechanized-Pipeline-Welding-Magnatec.pdf>

Kannayeram Gnanapandithan

ungelesen,
27.10.2016, 02:50:0927.10.16
an materials-welding
go with Bug O System with multiple torches

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Thu, Oct 27, 2016 at 9:24 AM, 'Neilashkumar' via Materials & Welding <material...@googlegroups.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (materials-welding@googlegroups.com) Add cleanup rule | More info

Dear Lakshman,

Good morning, as told by Pradip sir it's has to be root weld by GMAW-STT, followed by  SAW -Machine Welding column and boom with roller bed both in site or shop.
Since 3meter OD little bit difficult with Mechanisation process, and I have practical experience with Magna tech and lone star machine up to 48 inch only.
I don't see any external band for 3meter OD.
Even in machine welding in order to increase productivity you can choose Twin wire SAW process.
Further any clarification let me know to clarify.
P.NEILASHKUMAR 
Sent from my iPad
MOB : 966 551094590
             +91 9952110791
On 27-Oct-2016, at 6:40 AM, pgoswami <pgos...@quickclic.net> wrote:

Hi Lakhsman,

 

Both the processes are popular choices for pipeline welding. Mechanization  is the key. In general controlled surface transfer process e.g. STT or RMD are very conveniently used for long pipeline welding projects to cut down the production time and defect rates.

 

The attached documents provide some insights to such projects. Use the info at your discretion.

 

Thanks.

 

 

 

Pradip Goswami, P.Eng,IWE
 Welding & Metallurgical Engineering Specialist ,

ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAYAAAAAAAAAOT5XfyRhstKvyeqQRSrfFXCgAAAEAAAALpHkqFntblOtVlMJ77H09YBAAAAAA%3D%3D%40quickclic.net.

For more options, visit https://groups.google.com/d/optout.
<Mechanized-Pipeline-Welding-Magnatec.pdf>

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/0FD338FD-704C-442D-9BF4-6058762CE43D%40yahoo.com.

Lakshman Kumar. B

ungelesen,
27.10.2016, 06:24:3027.10.16
an material...@googlegroups.com

Dear Mr. Pradip And all friends…

 

Thanks a lot for sharing your valuable inputs, and really it’s a great learning and good understanding also….

 

Further I would like to bring to your notice for the following key parameters…

(please see the images also and pls be informed that it is of water pipe line and cant able to correlate with Oil & Gas Cross country pipe lines) the following limitations we have …

 

1.       Pipe are not in exact round shape and most of the time pipes internal will be supported by spider pipes (bracings) to retain its shape, however those will be removed during execution time. Here 120 Inch dia (3000Mtr dia) with a thickness of 16/18 mm – D/T is almost 190…

 

Hence internal / external fitup clamps are not possible.

Edge preparation at site is not feasible, and we have a limitation to restrict to factory made bevel or bevel preparation by free hand ( not that much accurate)

 

 

2.       Pipe will be laid in the trench one after one – (like as O&G it is not welded outside the trench and lowering the pipe line with side booms) – after completing one pipe welding another pipe will be laid and will continue further…

3.       Hence pipe are directly laying in the trench, we didn’t have much clearance under the pipe

 

Hence big weld heads are not possible to use.

We can’t able to go for full automation like as CRC Evans and all (earlier I worked in Reliance and in CRC welding)

 

4.       Like as O&G – alignments are not too much straight, and didn’t have free ROU clearances –

O&G lines has to laid far from villages and dense areas, where as Water lines have to laid near to villages and cities by connecting all the areas.

Like as in O&G or for full automation – we can’t provide the clear work front.

 

Water lines have the above limitations and so only we should be particular about the process…

Any way I understood Any of  the process can be implemented.

 

Thanks & Regards,

Lakshman Kumar B,

+91 9440031459.

 

pipe laying.jpg
Pipes with spiders.jpg
laid pipe line.jpg
pipe line welding.jpg
Laying of pipe.jpg 2.jpg
Laying of pipe.jpg
Big dia pipe.jpg

Hemant W Joshi

ungelesen,
02.11.2016, 06:18:2602.11.16
an material...@googlegroups.com

The issue of using IS 2062 plate for the pipes as has being enquired rihghty so by mr. Nautiyal remains unanswered. Can we get an idea about it?


For more options, visit https://groups.google.com/d/optout.


----------------------------------------------------------------------------------------------------------
Information transmitted by this E-MAIL is intended only for the use of the addressee(s) and contains information that is privileged, confidential or exempt from disclosure under applicable law. If you are not the intended recipient or it appears that this mail has been forwarded to you without proper authority, you are notified that any use or dissemination and or copying of this email in any manner is strictly prohibited and you are requested to delete this e-mail immediately.
Communicating through e-mail is not secure and capable of interception and delays. Any one communicating with TATA Consulting Engineers Ltd., and / or its subsidiaries or associates or group companies by e-mail accepts the risks involved and their consequences.
While this e-mail has been checked for all known viruses, the addressee should also scan for viruses and notify the originator of e-mail.
---------------------------------------------------------------------------------------------------------

Gopi Krishna Banerjee

ungelesen,
03.11.2016, 06:42:3203.11.16
an material...@googlegroups.com

Sir 

It is possible that if you use Pulsed MIG for Root Run only and Subsequent Run by FCAW Process for this Projects. 

G. K. Banerjee.

NAGPUR.


To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.


----------------------------------------------------------------------------------------------------------
Information transmitted by this E-MAIL is intended only for the use of the addressee(s) and contains information that is privileged, confidential or exempt from disclosure under applicable law. If you are not the intended recipient or it appears that this mail has been forwarded to you without proper authority, you are notified that any use or dissemination and or copying of this email in any manner is strictly prohibited and you are requested to delete this e-mail immediately.
Communicating through e-mail is not secure and capable of interception and delays. Any one communicating with TATA Consulting Engineers Ltd., and / or its subsidiaries or associates or group companies by e-mail accepts the risks involved and their consequences.
While this e-mail has been checked for all known viruses, the addressee should also scan for viruses and notify the originator of e-mail.
---------------------------------------------------------------------------------------------------------

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a1fd5667b6644a788fa366c75d04e5dd%40MUMEXG02.TCE.COM.
Allen antworten
Antwort an Autor
Weiterleiten
0 neue Nachrichten