Welding of SB729 UNS NO8020

167 views
Skip to first unread message

rajesh s. mhaske ,Engineer Welding ,PUNE,INDIA

unread,
Apr 22, 2016, 1:00:35 AM4/22/16
to Materials & Welding
Dear All
Please provide the guidlines of welding of SB 729 and B462 (alloy 20 ),i have selected the ER320LR and ERNiCrMo-3 for welding of Alloy 20, is it correct ?

plz reply

pgoswami

unread,
Apr 22, 2016, 10:23:43 AM4/22/16
to material...@googlegroups.com

Hi Rajesh,

If it involves welding or Alloy 20 to same , them ER320LR is the matching & ideal consumable. ERNiCrMo-3  will be over matching as well  as over priced. This filler could be used for dissimilar joints between alloy 20 and other alloys. Please seethe attachment for more details.

 
Thanks.

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299
pgos...@quickclic.net
pradip....@gmail.com
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/9083c67a-d80a-41fb-bfc0-26c275834801%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
ALLOY-20_FI_US_EN.pdf

Kannayeram Gnanapandithan

unread,
Apr 22, 2016, 10:53:08 PM4/22/16
to materials-welding

rajesh s. mhaske ,Engineer Welding ,PUNE,INDIA

unread,
Apr 22, 2016, 10:53:51 PM4/22/16
to Materials & Welding
Dear sir,
Thank you very much for your reply.ER320 LR is not available in our area so can i use ERNiCr-3 for welding of alloy 20 ?

Kannayeram Gnanapandithan

unread,
Apr 23, 2016, 12:28:07 AM4/23/16
to materials-welding
no, u may use 317 which is readily available in the market

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY

On Sat, Apr 23, 2016 at 12:40 AM, rajesh s. mhaske ,Engineer Welding ,PUNE,INDIA <rajesh....@gmail.com> wrote:
Dear sir,
     Thank you very much for your reply.ER320 LR is not available in our area so can i use ERNiCr-3 for welding of alloy 20 ?
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

Vishwas Keskar Welding Manager WELDING

unread,
Jan 17, 2021, 10:05:45 PM1/17/21
to Materials & Welding

ER320LR is matching consumable . Weld with due care .
 ERNiCrMo-3  is aslo acceptable