% Ferrite & FN measurements of Duplex Stainless steel welds

1,256 views
Skip to first unread message

Mohammed Azharuddin

unread,
Aug 23, 2016, 12:27:07 AM8/23/16
to material...@googlegroups.com, Pradip Goswami

Dear Experts,


We have performed qualification on Duplex stainless steel BM UNS 31803 welded to itself with filler ER2594. Shielding gas AR+2% nitrogen


Ferrite measurements of welds were carried out as per ASTM E562 and AWS A4.2.


Client has rejected these values as the correlation is not appropriate.See below reported values and client comment.


From client point of view ,It should have been like VOL % FRRITE = 70% FN VALUE.


Your valuable advise will help us to save this WPS from being rejected.


Many Thanks


Regards,

Mohammed Azharuddin

Mohammed Azharuddin

unread,
Aug 23, 2016, 12:31:01 AM8/23/16
to material...@googlegroups.com, Pradip Goswami
Reported values and client comments attached

I believe that 70%FN = VOL% FERRITE is a rule of thumb 

Actual correlation must be established from the measurements during PQR qualification


Inline images 1

Inline images 2

Inline images 3

Harish Kannepalli

unread,
Aug 23, 2016, 12:33:45 AM8/23/16
to material...@googlegroups.com

Please change your ferrite meter readings to %ferrite. Your problem solved.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEeeqaKkHHhBuUFxq5QX32g5vOV4JrYdb1X0fWAyf9qSrZHN0w%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

pgoswami

unread,
Aug 24, 2016, 11:33:41 PM8/24/16
to humai...@gmail.com, material...@googlegroups.com

Mr Azharuudin,

 

Your client is correct. The established formula for conversion is : % Ferrite= 0.7 x Ferrite No(FN)  or FN= 1.4 X % Ferrite.

 

Please see the highlighted texts in the attached documents of Fisher Ferrito scope for your information. Up to 28-30  abstract values both FN & % Ferrite runs equal. At higher values the FN is more in number that %Ferrite.

 

If you look at the ferritoscope MP-30  training document, when you plot the lines intersecting the centerline of the curve(Page-4), it’s clearly visible at higher % Ferrite values, the numerical values of  Ferrite No(FN) is more.

 

Also it would be advisable to cross check the Lab reading (computed as per ASTM E-562) with Fisher Ferrito scope also.  As claimed in the  Ferrito scope catalogue(marked with a arrow)  results could be correlated both in % Ferrite  7 Ferite No.

 

Use these information to straighten out the calculation and get your PQR through.

 

Also a question, what prompted you use Super Duplex Welding filler wire for DSS UNS-31803??  Appreciate  your response.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 

 .


From: Pradip Goswami [mailto:pradip....@gmail.com]
Sent: Wednesday, August 24, 2016 9:49 AM
To: Anasua Goswami
Subject: Fwd: Re: % Ferrite & FN measurements of Duplex Stainless steel welds

 

---------- Forwarded message ----------
From: "Mohammed Azharuddin" <humai...@gmail.com>
Date: Aug 24, 2016 3:19 AM
Subject: Re: % Ferrite & FN measurements of Duplex Stainless steel welds
To: "Pradip Goswami" <pradip....@gmail.com>
Cc:

Dear Mr. Pradip,

 

Please see attached client specification.

 

We reported ferrite in both vol% and FN value.But the correlation what client is asking ( 70% FN VALUE= VOL% FERRITE ) we are unable to get it.Moreover it is a thumb rule I believe.

 

Thanks

Mohammed Azharuddin

 

On 23 August 2016 at 19:39, Pradip Goswami <pradip....@gmail.com> wrote:

Could you scan and email the entire spec.Your client is correct asking ferrite to be reported in volume or % ferrite. Thx

 

On Aug 23, 2016 12:29 AM, "Mohammed Azharuddin" <humai...@gmail.com> wrote:

Reported values and client comments attached

 

I believe that 70%FN = VOL% FERRITE is a rule of thumb [pgoswami] --- This is not a rule of thumb. This conversion is arrived at after conducting numerous tests and correlations of numerous data on weld  ferrite content.

 

Actual correlation must be established from the measurements during PQR qualification

 

 

Inline images 1

 

Inline images 2These readings are wrong. Please see the explanations above.

 

Inline images 3

image004.gif
image005.gif
image006.gif
BROC_FMP30_FERITSCOPE_902-039_en.pdf
20563661-Feritescope-MP30-Training.pdf

Mohammed Azharuddin

unread,
Aug 25, 2016, 2:09:56 AM8/25/16
to pgoswami, material...@googlegroups.com
Dear Mr. Pradip,

Many thanks for your valuable suggestion and references.

It was suggested by Consumable manufacturer  to use Super duplex filler metal as we were unable to pass corrosion test required by SAES-W-016.

Regards,
Mohammed Azharuddin

On 25 August 2016 at 06:32, pgoswami <pgos...@quickclic.net> wrote:

Mr Azharuudin,

 

Your client is correct. The established formula for conversion is : % Ferrite= 0.7 x Ferrite No(FN)  or FN= 1.4 X % Ferrite.

 

Please see the highlighted texts in the attached documents of Fisher Ferrito scope for your information. Up to 28-30  abstract values both FN & % Ferrite runs equal. At higher values the FN is more in number that %Ferrite.

 

If you look at the ferritoscope MP-30  training document, when you plot the lines intersecting the centerline of the curve(Page-4), it’s clearly visible at higher % Ferrite values, the numerical values of  Ferrite No(FN) is more.

 

Also it would be advisable to cross check the Lab reading (computed as per ASTM E-562) with Fisher Ferrito scope also.  As claimed in the  Ferrito scope catalogue(marked with a arrow)  results could be correlated both in % Ferrite  7 Ferite No.

 

Use these information to straighten out the calculation and get your PQR through.

 

Also a question, what prompted you use Super Duplex Welding filler wire for DSS UNS-31803??  Appreciate  your response.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 

 .

Pieper QSI

unread,
Aug 25, 2016, 7:11:25 AM8/25/16
to material...@googlegroups.com

Dear Pradip,

 

I think Mr. Azharuudin is working according to a Shell or Total specification (or other oil company), some of those specifications require Super Duplex Filler metal for the root pass.

 

Met vriendelijke groeten / Best Regards,

 

Herman Pieper

QA-QC Inspector / CSWIP + IWI-C Welding Inspector / IWT / Materials Expert

 

Logo_nieuw_vectorized 60%

Job van der Havestraat 6

8384 DB, Wilhelminaoord

Cell: +31 6 51691215

 

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAYAAAAAAAAAOT5XfyRhstKvyeqQRSrfFXCgAAAEAAAAPKLD384X%2BJDvDJ4rAuwEEsBAAAAAA%3D%3D%40quickclic.net.

image002.gif
image003.gif
image004.gif
image005.png
Reply all
Reply to author
Forward
0 new messages