Dear sir,

In clean out door in tank we found welding not sufficient after PWHT.(A 537 CL1)
SO, now need to welding again . PWHT again doing or can avoid it by which code ?

Regards
krisanu bhunia
 

syed moinul hasan

unread,
Jul 16, 2016, 9:16:27 AM7/16/16
to material...@googlegroups.com
After PWHT, if the welding is added , that means  you have to discard residual stresses which occured  due to additional  welding.
Hence, you have to go for Re-PWHT , refernce ASME 31.3

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMZth3qmH8a3w0Efd96-M12HsymvR61YRPz18j1nOFpdZME9PQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

José Juan Jiménez Alejandro

unread,
Jul 16, 2016, 11:27:33 PM7/16/16
to material...@googlegroups.com
According to Section VIII Div. 1 BPVC ASME, you can do some kind of repracion after the PWHT welded, but this only applies to materials P1 and P3 number and for some thicknesses, which clearly defines the code.




For more options, visit https://groups.google.com/d/optout.



--

Ing. Jose Juan Jimenez Alejandro

Cel. 8116171750

Skype: jjjimeneza

Krisanu Bhunia

unread,
Jul 17, 2016, 6:59:31 AM7/17/16
to Materials & Welding
Thanks, but is it possible to avoid PWHT ?

José Juan Jiménez Alejandro

unread,
Jul 17, 2016, 9:12:24 PM7/17/16
to material...@googlegroups.com
It is assumed that in making this repracion of welding after the PWHT is no longer necessary to repeat again PWHT, but this is only for numbers P1 and P3 under certain thicknesses with the Building Code BPVC ASME Section VIII Div. 1

At this point I do not have exactly the reference code, you send it later for your review it thoroughly.

2016-07-17 0:18 GMT-05:00 Krisanu Bhunia <krisan...@gmail.com>:
Thanks, but is it possible to avoid PWHT ?
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

For more options, visit https://groups.google.com/d/optout.

Krisanu Bhunia

unread,
Jul 18, 2016, 9:17:08 AM7/18/16
to material...@googlegroups.com
Dear Sir,

Please mention where it is in See viii ?

You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/uHRzkNOaGNw/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-weld...@googlegroups.com.

To post to this group, send email to material...@googlegroups.com.

TC Kwa

unread,
Jul 18, 2016, 9:10:01 PM7/18/16
to material...@googlegroups.com

ishwar kumar

unread,
Jul 20, 2016, 11:58:38 AM7/20/16
to material...@googlegroups.com
Dear experts

My query is what happens if the soaking time during PWHT is increased beyond the specified minimum time. I know section 8 days minimum soaking time only.

Suppose if required soaking time is 2.5 hours and actual soaking time is 5 hours

Regards
Ishwar Dhiman
Cswip 3.1,ASNT NDT Level-II

Sent from my iPhone

Prakash Hegde

unread,
Jul 21, 2016, 4:26:18 AM7/21/16
to material...@googlegroups.com
Hi!
Selecting the Time and temp for PWHT is important  as it affetcts the mechanical properties
For which LM (Larsen Miller parameters ) helps
Increase in soaking time beyond certain limit deteriorates the mechanical properties
e.g. As per LM parameters  PWHt soaking temp of 650C with  2hrs soaking time is equivalent of 9hrs soaking time at 620C (even though code says for P1 soaking temp min 593c to below AC 1 )
Therefore you can imagine the importance of PWHT temp and time
Regards
Hegde




--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.

To post to this group, send email to material...@googlegroups.com.

Kannayeram Gnanapandithan

unread,
Jul 22, 2016, 1:01:51 AM7/22/16
to materials-welding
u should have simulated before taking up job. It is normally done by expecting  weld repairs after SR

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

To post to this group, send email to material...@googlegroups.com.

TDK YOKESH

unread,
Jul 23, 2016, 6:32:56 AM7/23/16
to material...@googlegroups.com

Hi ,
Well ,all your residual stresses would have been removed but check for the hardness value and  impact toughness if it  is an criteria . Basically your mechanical properties of the weld are affected .


ishwar kumar

unread,
Jul 26, 2016, 5:31:26 AM7/26/16
to material...@googlegroups.com
image1.JPG

Sent from my iPhone
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

José Juan Jiménez Alejandro

unread,
Jul 27, 2016, 1:50:49 AM7/27/16
to material...@googlegroups.com
BPVC ASME Section VIII Div 1, allows welding after the PWHT, but only for materials P1 and P3 and only certain thickness, but remember that this code is only for new equipment, not for equipment being repaired, if this is your building code ahead !.


For more options, visit https://groups.google.com/d/optout.

Krisanu Bhunia

unread,
Jul 27, 2016, 2:56:40 AM7/27/16
to material...@googlegroups.com
thank you, A537 CL1 is P1 marital but which thickness can do welding and which clause it is mention     

You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/uHRzkNOaGNw/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-weld...@googlegroups.com.

To post to this group, send email to material...@googlegroups.com.

José Juan Jiménez Alejandro

unread,
Jul 27, 2016, 11:02:20 PM7/27/16
to material...@googlegroups.com
This information is gold, few people know.
Regards!.


For more options, visit https://groups.google.com/d/optout.
UCS-56.pdf

Perumal Govindan

unread,
Jul 30, 2016, 2:50:46 AM7/30/16
to material...@googlegroups.com
Mr Jose is correct

With Kind Regards

P Govindan



George Dilintas

unread,
Aug 7, 2016, 6:09:40 AM8/7/16
to Meghanadh K
Creep may occur 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2888C0BE-2391-482F-95BA-0A98DEA102FE%40gmail.com.

For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

untraceablenator

unread,
Aug 8, 2016, 5:56:37 AM8/8/16
to Materials & Welding
Dear Ishwar,

You have simulated the welding & parent material with 2 cycle of PWHT.
This may effect your mechanical properites (specially impact & hardness), kindly take the test piece & simulate what you have carried out on the job.

The job can be accepted, If the test result meets the code requirement.