UT in lieu of RT

1,496 views
Skip to first unread message

Josnit

unread,
Sep 7, 2013, 1:18:18 AM9/7/13
to material...@googlegroups.com
Dear Experts,

For vessels constructed as per ASME Section VIII Div.1 is it acceptable to carry out manual UT in lieu of RT?. Reference to which clause, it should be done?.

Regards,
Josnit 

veera raghava kommisetti

unread,
Sep 7, 2013, 4:39:29 AM9/7/13
to material...@googlegroups.com
No, only recordable UT is allowed (in other words PA or ToFD


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

CHINTUKUMAR GANDHI

unread,
Sep 7, 2013, 4:52:07 AM9/7/13
to material...@googlegroups.com
Please refer the extract of UW-11(a) (7).

Ultrasonic examination in accordance with UW-53 may be substituted for radiography for the final
closure seam of a pressure vessel if the construction of the vessel does not permit interpretable radiographs in accordance with Code requirements. The absence of suitable radiographic equipment shall not be justification for such substitution.

Thanks & regards,


C. R. GANDHI


From: veera raghava kommisetti <kommi...@gmail.com>
To: material...@googlegroups.com
Sent: Saturday, September 7, 2013 2:09 PM
Subject: Re: [MW:18604] UT in lieu of RT

Steven Teo

unread,
Sep 7, 2013, 8:53:54 PM9/7/13
to material...@googlegroups.com
Seek equipment owner's approval for the use of recordable UT to replace RT (at least partially) to avoid the harzradous ionizing radiation method other than odd hours RT application. International Standard ASME 2235-9 Case allowed this. PAUT/TOFD procedure and operator qualification must be approved. UT has better advantages than RT in detecting severe type defects...ie..planar shape.
What concerned owners and certifying authoirty is NDT malpractises in steelwork industries. This can also happen in RT method too.

From: CHINTUKUMAR GANDHI <cgand...@yahoo.com>
To: "material...@googlegroups.com" <material...@googlegroups.com>
Sent: Saturday, 7 September 2013, 17:52
Subject: Re: [MW:18605] UT in lieu of RT
Please refer the extract of UW-11(a) (7).

Ultrasonic examination in accordance with UW-53 may be substituted for radiography for the final
closure seam of a pressure vessel if the construction of the vessel does not permit interpretable radiographs in accordance with Code requirements. The absence of suitable radiographic equipment shall not be justification for such substitution.

Thanks & regards,


C. R. GANDHI

From: veera raghava kommisetti <kommi...@gmail.com>
To: material...@googlegroups.com
Sent: Saturday, September 7, 2013 2:09 PM
Subject: Re: [MW:18604] UT in lieu of RT
No, only recordable UT is allowed (in other words PA or ToFD
On Sat, Sep 7, 2013 at 9:18 AM, Josnit <nithind...@gmail.com> wrote:
Dear Experts,

For vessels constructed as per ASME Section VIII Div.1 is it acceptable to carry out manual UT in lieu of RT?. Reference to which clause, it should be done?.

Regards,
Josnit 
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsu...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to mailto:materials-welding%2Bunsu...@googlegroups.com.
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

sathishkumar R

unread,
Sep 8, 2013, 4:34:27 AM9/8/13
to material...@googlegroups.com
Hi Josit..! Good day..!!

As an alternative to the RT, the weld metal thickness > 13 mm (above ) may be Ultrasonically examined as per the requirements of 7.5.5 of ASME VIII Div 2 

Ref : VIII Div 1, UW51 (a) (4)

ASME VIII Div 2 - 7.5.5 : Written procedure required as per Section V, Article 4, Mandatory Appendix VIII ( which covers only automated or semi automated scanning )

Conclusion: Manual UT not allowed. Try TOFD, if t>13mm

For Info: ASME 2235-9 case has been removed and incorporated in the code book itself.

Hope it helps you..!!

prem nautiyal

unread,
Sep 8, 2013, 5:39:13 AM9/8/13
to material...@googlegroups.com
Hi 

As per ASME Section VIII Div.1, 2013 edition,
UW-51(a)(4), the Minimum plate thickness for UT examination has been lowered from (1/2 inch) 13mm to 6mm (1/4 inch).

Now a manufacturer may perform UT in lieu of RT for all welds in material 6mm and greater in thickness using current UT technology such as Linear Phased Array Ultrasonic Testing.

Regards

Prem Nautiyal
9769316004


¨


From: sathishkumar R <sathi...@gmail.com>
To: material...@googlegroups.com
Sent: Sunday, September 8, 2013 2:04 PM
Subject: [MW:18614] Re: UT in lieu of RT

--

george....@gr.bureauveritas.com

unread,
Sep 9, 2013, 7:47:18 AM9/9/13
to material...@googlegroups.com

Only for the final seem and when not possible to have access to place the film.
On a top of that a Code Case is applicable

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor
    API 510 Inspector
    Prelude FLNG ASME Subject Matter Expert

    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    Korea cell phone: +82 10 2777 8922

Inactive hide details for Josnit ---07/09/2013 11:05:54---Dear Experts, For vessels constructed as per ASME Section VIII Div.1 Josnit ---07/09/2013 11:05:54---Dear Experts, For vessels constructed as per ASME Section VIII Div.1 is it acceptable to

--

To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at


http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit
https://groups.google.com/groups/opt_out.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Sathishkumar R

unread,
Sep 9, 2013, 11:09:20 AM9/9/13
to material...@googlegroups.com
Dear sir, 

  In my opinion, VIII Div 1 or Code case 2235 - 10, not mentioned about final seam. If you provide any reference, that could help me lot.

 As per my understanding, it applicable for ALL WELDS ( t = 6 mm and above as per 2013 Edition ).  Please correct me, if I am wrong

VIII Div 1 :

Inline image 1

Code case 2235 - 10 :

Inline image 2




You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/t_BxZj8S_Qs/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-weld...@googlegroups.com.

For more options, visit https://groups.google.com/groups/opt_out.



--
Thanks & Regards

 

 

cid:image001.jpg@01CE2FA6.38DDCE20

SATHISHKUMAR R Third Party Inspector - Trainee(Mechanical / Welding), Velosi Qatar 

E sathi...@gmail.com   Mob| +974 6615 2072

 

T| +974-4435.2850    EXT| 107   F| +974-4435.2819   W| www.velosi.com

A| Office Nos. 1,18 & 20 Eli France Cafè Building, Ramada Junction, Salwa Road, P.O. Box 3408, Doha, Qatar




image.png
image001.jpg
graycol.gif
image.png

pgoswami

unread,
Sep 9, 2013, 10:10:19 PM9/9/13
to material...@googlegroups.com, sathi...@gmail.com
Hi Satish,
 
Please see the code case along with discussion blogs on the same issue. The emphasis is on digital UT and state of art UT like TOFD  and Phased Array.
 
Thanks. 
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 
http://www.vsonomatic.com/publications/experience_with_code_cases.pdf

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Sathishkumar R
Sent: Monday, September 09, 2013 11:09 AM
To: material...@googlegroups.com
Subject: Re: [MW:18619] UT in lieu of RT

image.png
image.png
graycol.gif
image001.jpg
Use of Ultrasonic Examination in Lieu of Radiography.pdf
Reply all
Reply to author
Forward
0 new messages