Can anyone suggest what is the maximum single layer thickness that can be achieved in SAW hardfacing. 

Dinesh Somwanshi

unread,
Sep 2, 2019, 10:26:12 AM9/2/19
to materials-welding

Generally its coming 3-4 mm.

On Sep 1, 2019 10:14 AM, "Weldbro" <itsashi...@gmail.com> wrote:
Can anyone suggest what is the maximum single layer thickness that can be achieved in SAW hardfacing. 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/39f9b768-7fa6-47d9-a09c-4aaf59a22e19%40googlegroups.com.

Ashish Walia

unread,
Sep 2, 2019, 11:05:27 AM9/2/19
to material...@googlegroups.com
thanks for reply dinesh but i have heard of some ways by which even 12mm is achieved and i am curious to find out how is that possible i have myself reached upto 6mm

On Mon, Sep 2, 2019 at 4:26 PM Dinesh Somwanshi <som...@gmail.com> wrote:

Generally its coming 3-4 mm.

On Sep 1, 2019 10:14 AM, "Weldbro" <itsashi...@gmail.com> wrote:
Can anyone suggest what is the maximum single layer thickness that can be achieved in SAW hardfacing. 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/XQfxQe8wT9E/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAELgRrVsVVeqsEnpyu9bRz-S4-%3DLsTjPKqJJ%2BpPQ6FrYsvZd-w%40mail.gmail.com.

Ramin Kondori

unread,
Sep 2, 2019, 11:56:13 PM9/2/19
to material...@googlegroups.com
Dear WeldBro,

Generally speaking, by using larger-diameter wires, increasing the overlap (much above normal 50%), lowering the travel speed, having a higher voltage and so forth, you can achieve layers with higher thickness. Of course, it all depends on the qualification test results which will eventually put a limit on it.

Regards   
Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


Kannayeram Gnanapandithan

unread,
Sep 3, 2019, 12:29:01 AM9/3/19
to materials-welding
Connect the Electrode in Negative terminal, u will get higher thickness. 

Amitabh Bhattacharya

unread,
Sep 4, 2019, 11:15:49 PM9/4/19
to material...@googlegroups.com
Hi Ashish,
Attached a FAQ document on Hard facing for your review. Hope this helps..
Regards
Amitabh 

FAQ-hardfacing.pdf
Reply all
Reply to author
Forward
0 new messages