Where to we find DIN wire IQI Thickness?
Which standard is deals about DIN wire IQI Thickness?
Where to refer?

Ramachandran M S

unread,
May 30, 2010, 4:23:57 AM5/30/10
to material...@googlegroups.com
Wire IQI
Used to assess sensitivity ; quality of technique 
Pl refer DIN 54109 (1962); ISO 1027
Wire set 1-7; set 6-12; set 10-16 (1,7,6,12,10,16 represent wire numbers)
3 sets - each set having 7 wires (overlapping with adj set) arranged in GP
usually 2% or lesser value of sensitivity is required for general applications
Smaller no 1% indicates higher sensitivity -critical applications

wire dia          wire No
   mm                        
   3.2 ...............  1 
   2.5  ............... 2
   2.0  ............... 3
   1.6   ...............4
   1.25 ...............5
   1.0   ...............6
    0.8  ...............7
---------------------------    
    1.0   ..............6
    0.8  ...............7  
    0.63 ...............8
    0.50................9
    0.40..............10
     0.32..............11
    0.25...............12
-----------------------------
    0.40..............10
    0.32..............11
    0.25..............12
    0.20 .............13
    0.15 .............14  
    0.125............15
    0.10 .............16
  ---------------------------


Regds
MSR
--------------------------------------------------------------------------------------
--------------------------------------------------------------------------------------------------------------------------------------

Samimi Mottagi, Alireza

unread,
May 30, 2010, 5:15:28 AM5/30/10
to material...@googlegroups.com
Hi dear
You can find your requirements in DIN EN 462(1,2,3,4,5,6)

Best regards

Dear All

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to
materials-weld...@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.

__________ Information from ESET NOD32 Antivirus, version of virus
signature database 5155 (20100530) __________

The message was checked by ESET NOD32 Antivirus.

http://www.eset.com

__________ Information from ESET NOD32 Antivirus, version of virus
signature database 5155 (20100530) __________

The message was checked by ESET NOD32 Antivirus.

http://www.eset.com

rutvik dixit

unread,
May 30, 2010, 6:10:54 AM5/30/10
to material...@googlegroups.com
I am not sure, but please try EN 462-1.

With Regads,
Rutvik
Sr.Surveyor
TATA Projects Ltd.

--- On Sun, 30/5/10, Srinivas Engr <srinivas...@gmail.com> wrote:

> From: Srinivas Engr <srinivas...@gmail.com>
> Subject: [MW:5292] DIN Wire IQI Thickness

AGUSTIN JIMENEZ

unread,
May 30, 2010, 9:55:43 AM5/30/10
to material...@googlegroups.com, INSPECTORES DE EQUIPOS ESATICOS
Hi Srinivas.
You can revised in ASME Section 5 Article 2 / T-233 Image Quality Indicator (IQI) Design, API 1104 / 11.1.5 Selection of Image Quality Indicators (IQI), ASTM E 747 or ISO 1027 too.
I hope that it information was utility.
 
Best regards.
Agustin Jimenez


De: Srinivas Engr <srinivas...@gmail.com>
Para: Materials & Welding <material...@googlegroups.com>
Enviado: dom, mayo 30, 2010 2:20:00 AM
Asunto: [MW:5292] DIN Wire IQI Thickness

puneet takiar

unread,
May 30, 2010, 12:03:11 PM5/30/10
to material...@googlegroups.com
Dear srinivas,
refer ASME section V table 276 for sizes
 

puneet takiar
________________________________

----- Original Message ----
From: Srinivas Engr <srinivas...@gmail.com>
To: Materials & Welding <material...@googlegroups.com>

Dear All

--

Kale, Bhaskar M

unread,
May 30, 2010, 10:28:28 PM5/30/10
to material...@googlegroups.com, INSPECTORES DE EQUIPOS ESATICOS

Please see the attached file for the IQI details.

Please refer the table in attached file for the relation between different code set and wire number.

Please fill free to contact if any more details required.

Regards, Bhaskar kale

--
धन्यवाद,
भास्कर मनोहर काळे
+60149129098
IQI TABLE.pdf

manpreet

unread,
May 30, 2010, 10:55:02 PM5/30/10
to material...@googlegroups.com
Hi
Refer ASTM E747 for IQI radiography.

Regards
Manpreet Singh
Welding Engineer
Spiecapag

On Sun, 30 May 2010 14:10:38 +0530 wrote
--

To post to this group, send email to material...@googlegroups.com

To unsubscribe from this group, send email to materials-weld...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


PATEL

unread,
Apr 28, 2017, 2:34:50 AM4/28/17
to Materials & Welding
Dear sir
DIN ISO 10ISO16 WIRE JOB THK 11.1 CAP+2MM RT FILM NUMBER OF IQI SHOW 

Kunjal Patel

unread,
Apr 29, 2017, 1:23:06 AM4/29/17
to material...@googlegroups.com
10ISO16 WIRE
API-1104 JOB THK 11.1
API1104



PATEL KUNJAL  
INSPECTION ENGINEERSGS INDIA PVT LTD





The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/I36HrxlDnSQ/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/51666b0a-b280-4481-800a-e5b846e5f5df%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Reply all
Reply to author
Forward
0 new messages