measuring of the gap between edges of crack

20 views
Skip to first unread message

asghar...@gmail.com

unread,
Dec 13, 2020, 11:02:19 PM12/13/20
to Materials & Welding
Dear All.
Does any body have any experience about measuring of the gap between edges of crack especially for HIC or SWC? and which method would be useful?
Regards, 

albert anbarasan

unread,
Dec 14, 2020, 2:29:13 AM12/14/20
to Materials & Welding
Hi,

Please refer to NACE TM0284, for the measurement of cracks with respect to crack sensitivity ratio (CSR), crack length ratio (CLR), and crack thickness ratio (CTR).,



R Albert Anbarasan 




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/f7fbe2f6-94d9-41a3-9cf9-558a6d579c14n%40googlegroups.com.

Ali Asghari

unread,
Dec 14, 2020, 3:51:37 AM12/14/20
to material...@googlegroups.com
Dear Albert.
Actually, I need it for F.F.S (crack area based on chapter 7 of API579) and I am looking for a reliable NDT method to measure HIC/ or even SWC from one accessible side.
Regards,

You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/CK8GPQuhFE4/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1825678550.322649.1607920619021%40mail.yahoo.com.

SENTHILKUMAR SWAMINATHAN

unread,
Dec 14, 2020, 5:16:07 AM12/14/20
to material...@googlegroups.com
What is the thickness,  Bevel configuration and materials specn? 
PAUT is opot 


Regards, S.SENTHILKUMAR


Ali Asghari

unread,
Dec 14, 2020, 6:14:24 AM12/14/20
to material...@googlegroups.com
Dear Senthilkumar.
Actually, we want to scan base metal but in some situations,  crack grow to weld.
Regards,

SENTHILKUMAR SWAMINATHAN

unread,
Dec 14, 2020, 9:12:03 AM12/14/20
to material...@googlegroups.com
Yes, low hydrogen electrode behave like.  PAUT scan in transverse direction to weld on basematerial 

Regards, S.SENTHILKUMAR