PWHT

76 views
Skip to first unread message

Maulik Thakkar

unread,
Mar 1, 2016, 4:29:04 AM3/1/16
to Materials & Welding

Dear all,
I have two queries:
MOC: P8Gr1(SS347 internal)
PWHT on job with LAS is at 705+/-10 degree C for 10 hrs.
Available PQR: 700 degree C for 8 hrs.
Can I support same PQR for welding of SS347 internal which will undergo PWHT at 705+/- 10 degree C along with LAS???

Impact: not applicable for SS.

Second query:
Interpretation of QW407.1 (b).

Regards,
Maulik

sandeep vaghela

unread,
Mar 1, 2016, 7:03:27 AM3/1/16
to material...@googlegroups.com

We consider 80% aggregate time and temp.
As per qw-407.2 of qualify procedure.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFK0MUMCrJL9dRmq0Q%3DDEJpfNmP%3DJ%3DRmrTk4fzV7cjfUj7FKdw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Kannayeram Gnanapandithan

unread,
Mar 1, 2016, 7:03:45 AM3/1/16
to materials-welding
what is grade of LAS?, u can if it is P22

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY

--

Mohd Siraj

unread,
Mar 1, 2016, 7:46:16 AM3/1/16
to Materials & Welding
QW-407.2 according to which the PWHT time of PQR shall be at least 80% of the production welding time.

10Hr 80% is 8hr.hence it is accepted.

Maulik Thakkar

unread,
Mar 1, 2016, 8:15:55 AM3/1/16
to Materials & Welding

Dear sir,
Yes as per as time is concern PQR is accepted. Anyway 407.2 will be non essential variable for SS as impact is not require.

But same PQR had PWHT at 700 degree C. Heat treatment chart does not showing any range so only single value is available in PQR. Now as per 407.1 b specific temperature range is essential variable in case of P8. In same situation can I support PQR of 700 degree C for execution of production weld which will be PWHT at 705+/-10 degree C?

Regards,
Maulik
Welding engg.

On Mar 1, 2016 6:16 PM, "Mohd Siraj" <mohd...@gmail.com> wrote:
QW-407.2 according to which the PWHT time of PQR shall be at least 80% of the production welding time.

10Hr 80% is 8hr.hence it is accepted.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
Reply all
Reply to author
Forward
0 new messages