Ductile iron to carbon steel welding

296 views
Skip to first unread message

JIJILAL K M

unread,
Apr 21, 2016, 6:52:19 AM4/21/16
to material...@googlegroups.com

Dear Associates,


We are in requirement of  WPS & PQR  for welding a pipe support   ASTM A36 /Equivalent    to   Ductile Iron ASTM  A536 gr. 65-45-15 .

This is for  fire water system Shure joint welding . please refer attachments.

Much appreciated if you can support with relevant WPS & PQR for reference.


JIJILAL K.M. 
Thai Jurong Engineering Ltd,
KCE SPP Project,Thailand


Company catalog & Spec for shur joint.pdf
Trunnion support.pdf
UNIBRAZE ELECTRODE.pdf

Mohd Siraj

unread,
Apr 21, 2016, 11:36:03 PM4/21/16
to Materials & Welding

dili...@gmail.com

unread,
Apr 21, 2016, 11:36:13 PM4/21/16
to JIJILAL K M
Nickel electrode with slow preheat up to 200degC. Max interpass temp same. Maintain preheat for 1 hour. Cover with insulating blanket and let cool down

Sent from my BlackBerry 10 smartphone.
From: JIJILAL K M
Sent: Πέμπτη, 21 Απριλίου 2016 - 13:52
Subject: [MW:24726] Ductile iron to carbon steel welding

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHmEnHitavvOMaBveL0zQotmkyBK6TvwSL8xPwb4PRvVMfi%2BFA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Reply all
Reply to author
Forward
0 new messages