LAS P11 minimum required hardness for operation

253 views
Skip to first unread message

Devang Majithia

unread,
May 28, 2021, 1:27:13 AM5/28/21
to material...@googlegroups.com
Dear All,
Hope all are safe and doing good in this tough time.

36" LAS P11 steel is used in FCC Reactor O/H line with operating temperature of 500-530 Deg. C. Design temp. is 569 Deg. C. Creep temperature starts from 427 Deg. C as per API 571. Line in service for 10 yrs.

Insitu metallography is taken and noted to be with pearlitic structure disintegration and dissolved carbides in matrix (at 500X). Refer pic.
image.png
image.png

We noted hardness in the range of 105-120 BHN which appears to be quite low against generally noted 160-180 BHN. Baseline reading is not available. Hardness measurement done with a portable machine having angle compensation.

Request to kindly guide me on how much minimum hardness is acceptable for P11 material for such critical service?

Regards,
Devang Majithia

pgos...@rogers.com

unread,
May 30, 2021, 10:58:31 PM5/30/21
to material...@googlegroups.com, Devang Majithia

Hi Devang,

An operating temperature of 500-530 Deg C is fairly high for P11 steel. Though the design code provides the allowable stresses at that temperature I would say for that operating temperature range selection of   P22 steel would have been a better choice. In the context of the refineries 300 series is very common so as to have the thermal stability and desired machinal properties @ 500-530 Deg C, why it was not chosen ??

Having said those, the hardness values 100-125 BHN too low for these steels. As fabricated and PWHT-ed( if applicable) hardness readings of 150-180 HB would have been appropriate.

Materials degradations in the creep range can’t be concluded by hardness reading alone. The following additional inspections are warranted:

  • Signs of deformations , swellings on the lines
  • Replications for Creep Cracks/damages.

You may find additional guideline in API 571.

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Consulting Welding & Metallurgical Engineering  Specialist

Saudi Aramco Approved Designated Project  Welding Engineer(DPWR)

Qatar Petroleum Approved, SME-Materials & Corrosion Engineering.

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

 

From: material...@googlegroups.com <material...@googlegroups.com> On Behalf Of Devang Majithia
Sent: May 27, 2021 11:41 PM
To: material...@googlegroups.com
Subject: [MW:32392] LAS P11 minimum required hardness for operation

 

Dear All,

Hope all are safe and doing good in this tough time.

 

36" LAS P11 steel is used in FCC Reactor O/H line with operating temperature of 500-530 Deg. C. Design temp. is 569 Deg. C. Creep temperature starts from 427 Deg. C as per API 571. Line in service for 10 yrs.

 

In situ metallography is taken and noted to be with pearlitic structure disintegration and dissolved carbides in matrix (at 500X). Refer pic.

 

We noted hardness in the range of 105-120 BHN which appears to be quite low against generally noted 160-180 BHN. Baseline reading is not available. Hardness measurement done with a portable machine having angle compensation.

 

Request to kindly guide me on how much minimum hardness is acceptable for P11 material for such critical service?

 

Regards,
Devang Majithia

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFfyh2gCxWQUPCGUntAs6U9na2eAca8e9n5d3e9m0%3D8kScCeaA%40mail.gmail.com.


Virus-free. www.avg.com
image002.png
image004.png

Ramon Briceno

unread,
Jun 1, 2021, 2:44:40 AM6/1/21
to material...@googlegroups.com

Dear Devang,

This P11 material is already affected by creep, the microstructures reveal it.

It has accumulation of microstructural damages due to prolong operation (10 years) decreasing their load bearing capacity, with formation of Cr carbides at the grain boundaries and carbon dissolution in the matrix.

You have to notify the plant of the need to change that section of pipe affected by creep, due to the risk of sudden cracking, with operational consequences.

On the other hand, under normal conditions, the welding of P11 material (1 ¼ Cr - ½ Mo) should has maximum hardness of 225 HBN for service at high temperature operating.

A good solution is use the material P22 (2 ¼ Cr-1/2 Mo). Propose it.

 

Regards,

Ramon Briceno

http://www.linkedin.com/in/ramonbriceno-metalengineer

 

Sent from Mail for Windows 10

 

From: Devang Majithia
Sent: Friday, May 28, 2021 1:27 AM
To: material...@googlegroups.com
Subject: [MW:32392] LAS P11 minimum required hardness for operation

 

Dear All,

Hope all are safe and doing good in this tough time.

 

36" LAS P11 steel is used in FCC Reactor O/H line with operating temperature of 500-530 Deg. C. Design temp. is 569 Deg. C. Creep temperature starts from 427 Deg. C as per API 571. Line in service for 10 yrs.

 

Insitu metallography is taken and noted to be with pearlitic structure disintegration and dissolved carbides in matrix (at 500X). Refer pic.

 

We noted hardness in the range of 105-120 BHN which appears to be quite low against generally noted 160-180 BHN. Baseline reading is not available. Hardness measurement done with a portable machine having angle compensation.

 

Request to kindly guide me on how much minimum hardness is acceptable for P11 material for such critical service?

 

Regards,
Devang Majithia

--

james gerald

unread,
Jun 1, 2021, 11:08:19 PM6/1/21
to material...@googlegroups.com
It seems to be like softening (spheroidized carbides) due to exposure to high temperature. Creep is normally associated with voids in the grain boundaries as visible at high magnification and internal strengthening of grains.

Similar micrograph from API 571 is shown below


Inline image
Some snap shots from API 571 shown below.

Inline image

Thanks & Regards

J.Gerald Jayakumar