Whats the thickness shall be done with PWHT CS material as per B31.3 latest edition .
Here the joint is branch weld of high thickness weldolet with low thickness pipe.
BINOY L
QC
If both thickness are under 25mm (1”), the PWHT can be exempted if you preheat to 95 C (or 200F) minimum.
If the weldolet exceeds 25mm, you need PWHT at 595 ~ 650C for 1hr/25mm.
|
|
||
|
Feng Lu, Ph.D.
|
||
|
||
|
This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message. |
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-weld...@googlegroups.com.
To post to this group, send email to
material...@googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/CAKrfo%2BDDp29cSaJxULSRAPbqaYcSRgp%2BXmRzmU76c0XFQJorRg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
As per the attached requirement from B31.3.2014 edition PWHT tequirement .the thickness considered is the lesser of the two parts joining .
Does it means if one of the parent metal is of below 25 mm PWHT not required.?
BINOY L
QC Engineer-Mechanical
AGC.
Project:AFU KKIA Riyadh.KSA
I have checked this but for PWHT the minimum thickness is not given.
BINOY L
QC Engineer-Mechanical
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOwU13tQWAZMSoY5C1OXOqYQYDHrSwnGvHcOuBR6MJc153h4dA%40mail.gmail.com.
I have checked this but for PWHT the minimum thickness is not given.
BINOY L
QC Engineer-Mechanical
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOwU13tQWAZMSoY5C1OXOqYQYDHrSwnGvHcOuBR6MJc153h4dA%40mail.gmail.com.
As per b31. 3 latest no need of pwht for p no :1 I.e cs
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKrfo%2BBFw2yGYR20SzfvavkwRpBjtdhY1-opPwrVVms%3DHb7qLQ%40mail.gmail.com.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKrfo%2BAiHibM-vVQhjPMNER%3DLp2ATk1x1Tq7BPO765KxGpA48w%40mail.gmail.com.