Preheating and PWHT for B31.3 CS mtls

159 views
Skip to first unread message

Binoy Lonappan

unread,
Mar 23, 2016, 1:21:11 AM3/23/16
to materials-welding

Whats the thickness shall be done with PWHT CS material as per B31.3 latest edition .
Here the joint is  branch weld of high thickness weldolet with low thickness pipe.

BINOY L
QC
   

Lu, Feng

unread,
Mar 24, 2016, 12:08:31 PM3/24/16
to materials-welding

If both thickness are under 25mm (1”), the PWHT can be exempted if you preheat to 95 C (or 200F) minimum.

 

If the weldolet exceeds 25mm, you need PWHT at 595 ~ 650C for 1hr/25mm.

 

 

Zachry Group Logo

Feng Lu, Ph.D.
Metallurgy and Welding Engineer

Zachry Industrial, Inc.
527 Logwood
San Antonio, TX 78221

l...@zachrygroup.com
Office: 210.588.7818
Cell: 512 797 5777
Fax: 210.588.5037
www.ZachryGroup.com

This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKrfo%2BDDp29cSaJxULSRAPbqaYcSRgp%2BXmRzmU76c0XFQJorRg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Lalu Rajendran

unread,
Mar 24, 2016, 12:08:44 PM3/24/16
to material...@googlegroups.com
Hi,

As per ASME B31.3 Edition2014, there is the exception for PWHT for P1 Carbon steel materials. Please see the below extract.

Inline image 1

regards,
LALU

--

Binoy Lonappan

unread,
Mar 27, 2016, 12:02:13 AM3/27/16
to materials-welding

As per the attached requirement from B31.3.2014 edition PWHT tequirement .the thickness considered is the lesser of the two parts joining .
Does it means if one of the parent metal is of below 25 mm PWHT not required.?

BINOY L
QC Engineer-Mechanical
AGC.
Project:AFU KKIA Riyadh.KSA
   

On 26 Mar 2016 12:48 pm, "Binoy Lonappan" <bino...@gmail.com> wrote:

I have checked this but for PWHT the minimum thickness is not given.

BINOY L
QC Engineer-Mechanical
   

Binoy Lonappan

unread,
Mar 27, 2016, 12:02:52 AM3/27/16
to materials-welding

I have checked this but for PWHT the minimum thickness is not given.

BINOY L
QC Engineer-Mechanical
   

On 24 Mar 2016 7:08 pm, "Lalu Rajendran" <lal...@gmail.com> wrote:

Binoy Lonappan

unread,
Mar 27, 2016, 12:02:52 AM3/27/16
to materials-welding
heat treatment-1.png

Mathiyazhagan V

unread,
Mar 27, 2016, 1:06:52 PM3/27/16
to material...@googlegroups.com

As per b31. 3 latest no need of pwht for p no :1 I.e cs

Lalu Rajendran

unread,
Mar 27, 2016, 1:06:55 PM3/27/16
to material...@googlegroups.com
Please refer 331.1.3 Definition of Thicknesses Governing PWHT.

Thickness shall be considered for the joints after edge preparation. For dissimilar thickness, you should consider the thickness at bevel edges.

regards,
LALU


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Reply all
Reply to author
Forward