Hi team  
   What is welding electrodes need to used for rail welding CR210 material to S355jr 

Regards,

Sriram Srinivasan





sridhar cn

unread,
Sep 26, 2025, 5:49:44 AMSep 26
to material...@googlegroups.com
For welding CR210 rail steel to S355JR, you can use E 8018-C3, a low hydrogen electrode.
Pre-heat the joint (CR210) to 250-350  °C and maintain  a max. interpass temp of 300 °C. 
Optionally, use E312-16 (high alloy Cr–Ni electrode) for buttering the rail steel and complete 
with E 309L for a ductile joint.  
C Sridhar.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJwhjYsVCO_L_3h%2BvoS3ihWQgrfnnBO1VjzyS4r%3DzXz1%3De51rw%40mail.gmail.com.
Reply all
Reply to author
Forward
0 new messages