Dear Experts,

Kindly suggest me which filler wire best suitable for dissimilar metal pipe joints P22 to cs SA106 Gr B

Awaiting for your valuable answer
 
With Regards

Bijay Kumar Choudhury

ravi_...@rediffmail.com

unread,
Jul 8, 2012, 9:08:08 AM7/8/12
to material...@googlegroups.com
Dear Bijay,

It would be better to use carbon steel consumable ER 70 S2 followed by stress relieving of joint as per applicable code of construction.

Regards
Ravinder sharma

Sent on my BlackBerry® from Vodafone

From: Bijay <bkchou...@yahoo.com>
Date: Sun, 8 Jul 2012 03:56:53 -0700 (PDT)
Subject: [MW:14805] Filler wire for pipe alloy steel (P22) to cs (P1)

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

hany karica

unread,
Jul 8, 2012, 9:08:22 AM7/8/12
to material...@googlegroups.com
dear experience    
E9018 B3 used for welding p22 to A106

From: Bijay <bkchou...@yahoo.com>
To: "material...@googlegroups.com" <material...@googlegroups.com>
Sent: Sunday, July 8, 2012 3:56 AM

Subject: [MW:14805] Filler wire for pipe alloy steel (P22) to cs (P1)
--

Dinesh Babu

unread,
Jul 8, 2012, 9:20:10 AM7/8/12
to material...@googlegroups.com
Dear fre,

suitable filler Wire ER 90S - B3, pls refer in ASME sec IIC.

--

Zulfan

unread,
Jul 8, 2012, 9:20:56 AM7/8/12
to material...@googlegroups.com
Dear Bijay,

What process you are looking for? 

Thanks

Zulfan

The Lincoln Electric Singapore

--

c sridhar

unread,
Jul 8, 2012, 11:53:37 AM7/8/12
to material...@googlegroups.com
You can use E 7016 -A1 or E 7018-A1 for P22 to CS.
Alternatively, E 8016 -B2 or E 8018-B2 is also recommended.

sridhar.


From: hany karica <hany_...@yahoo.com>
To: material...@googlegroups.com
Sent: Sunday, 8 July 2012 6:38 PM
Subject: Re: [MW:14807] Filler wire for pipe alloy steel (P22) to cs (P1)

rahul m

unread,
Jul 10, 2012, 7:19:20 AM7/10/12
to material...@googlegroups.com
sridhar,
 how u selected these electrodes ? what made you to suggest those electrodes?
Reply all
Reply to author
Forward
0 new messages