Diameter qualified

908 views
Skip to first unread message

C L

unread,
May 6, 2014, 10:51:58 PM5/6/14
to material...@googlegroups.com
Hi,
I'm a bit confuse. Say if i have a WPS qualified for ALL DIAMETER. During WQT, the welder is tested with 6" diameter test coupon. 
After WQT, can the welder perform welding for 1.5" diameter pipe?

Can anyone clear my doubt?

Thanks

John Henning

unread,
May 7, 2014, 2:25:36 PM5/7/14
to material...@googlegroups.com

No.  See QW-452.3.

 

If tested on a 6 inch diameter coupon, he is qualified for a minimum diameter  of  2 -7/8 inch (73mm).  He/she is qualified to weld any greater diameter than the minimum.

 

John A. Henning

Welding & Materials

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

Lakshman

unread,
May 7, 2014, 8:25:41 AM5/7/14
to material...@googlegroups.com
No welder is not permited to do welding for 1.5inch dia pipe as per section IX QW 452.3

With regards,
Lakshman Kumar.B
09440031459.

From: C L
Sent: ‎07-‎05-‎2014 17:00

To: material...@googlegroups.com
Subject: [MW:20762] Diameter qualified

mrs...@yahoo.com

unread,
May 7, 2014, 9:00:47 AM5/7/14
to material...@googlegroups.com

Is it fillet weld or butt weld. You have to re qualifiy the welder for the small bore

Sent from Yahoo Mail on Android



From: C L <lchca...@gmail.com>;
To: <material...@googlegroups.com>;
Subject: [MW:20762] Diameter qualified
Sent: Wed, May 7, 2014 2:51:58 AM

--

James Cyrilandrew

unread,
May 7, 2014, 1:26:57 PM5/7/14
to material...@googlegroups.com
hi,
 WPS and WQT are two different documents, WPS always qualified for all diamter, only limited to thickness and other essential variable.
but for WQT see ASME Sec IX welder Performance section the essential variable is very clearly addressed in a table. if a welder welded in 6 inch pipe he can weld dia above 2 7/8 inch to unlimited. he cannot weld 1.5 inch.
-- 
Regards,
J.C.Andrews
QA/QC Engineer
Doha-Qatar.

--

rudolf saldanha

unread,
May 7, 2014, 9:47:53 AM5/7/14
to material...@googlegroups.com
Hi, 
Under which code are your referring to.
The range for thickness and diameter for WPS and WQT are different.

Regards

AHMAD&MOHAMAD REDA

unread,
May 12, 2014, 5:27:25 AM5/12/14
to material...@googlegroups.com
hi sir
Do not be confused
according to ASME IX QW-452.3 (copy attached) YOUR WELDER IS now qualified to weld from  2,7/8" to UN limited dia.
and according to the table if the welder tested
1-any dia. over 2,7/8" he is qualified to weld from  2,7/8" to UN limited dia.
2-any dia. from 1" to 2,7/8" ie(1" or 1,1/2") he is qualified to weld from  1" to UN limited dia.
3-any dia.less than 1" ie(1/2" or 3/4") he is qualified to weld from size welded to UN limited dia.
GROVE WELD DIAMETER LIMITS.doc

kannayeram gnanapandithan

unread,
May 12, 2014, 11:10:01 AM5/12/14
to materials-welding
Do not confuse with WPS and WPQR. Pipe dia restriction is only for welder not for WPS. Since ur welder is qualified in 6", he can not be permitted to do 1.5" dia pipe.

THANKS & BEST REGARDS
KG.PANDITHAN, AWS-CWI, CSWIP 3.1
CONSULTANT-WELDING & QUALITY


--
Reply all