Black dots on sdss welding

69 views
Skip to first unread message

Narayanan Kumar

unread,
Oct 11, 2022, 11:32:58 PM10/11/22
to material...@googlegroups.com
Dear Team,

Can you please explain about the black dots appears on SDSS GTAW Weld bead( ER 2594 )  with document backup for the causes 


Regards,

M.Kumar 

pgos...@rogers.com

unread,
Oct 12, 2022, 11:12:30 AM10/12/22
to material...@googlegroups.com

Hi Narayanan,

 

Please refer the discussions and the answers provided the following link. The spots may appear due to few issues:

  • Type of lubricants used during wire drawing of the GTAW filler wires. Typically oil based lubricants if used could generate such residues, while soap type lubricants  may not.
  • Surface finish of the SDSS. If the products are acid cleaned & pickled after manufacturing the chances of such welding dross would be less.

Irrespective of those facts, the discussions in this following link are worthwhile to look at.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

 

Black spots on DSS Weld Joints. (google.com)

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADTvyj%2B9Ti77s60HeABOGGgrcOeok0BG2nwCqMQQ8zrDqdyGyw%40mail.gmail.com.


Virus-free.www.avg.com

pgos...@rogers.com

unread,
Oct 12, 2022, 12:06:35 PM10/12/22
to material...@googlegroups.com

 

Hi Narayanan,

 

Please refer the discussions and the answers provided the following link. The spots may appear due to few issues:

  • Type of lubricants used during wire drawing of the GTAW filler wires. Typically oil based lubricants if used could generate such residues, while soap type lubricants  may not.
  • Surface finish of the SDSS. If the products are acid cleaned & pickled after manufacturing the chances of such welding dross would be less.

Irrespective of those facts, the discussions in this following link are worthwhile to look at.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

 

Black spots on DSS Weld Joints. (google.com)

From: material...@googlegroups.com <material...@googlegroups.com> On Behalf Of Narayanan Kumar
Sent: October 11, 2022 9:31 AM
To: material...@googlegroups.com
Subject: [MW:33587] Black dots on sdss welding

 

Dear Team,

--

https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADTvyj%2B9Ti77s60HeABOGGgrcOeok0BG2nwCqMQQ8zrDqdyGyw%40mail.gmail.com.


Virus-free.www.avg.com

james gerald

unread,
Oct 16, 2022, 11:16:31 PM10/16/22
to material...@googlegroups.com
Will cleaning the Filler Rod and Joint using a solvent like Acetone will solve this problem.