Water Requirements for Hydrotest

1,310 views
Skip to first unread message

Manish Kumar

unread,
Sep 18, 2020, 7:38:49 AM9/18/20
to material...@googlegroups.com
Dear Sir,
I want to know that which type of water is used for Hydrotest in stainless steel piping and equipment. Please advise as per relevant code and standard.




Vishwas Keskar

unread,
Sep 18, 2020, 8:08:51 AM9/18/20
to material...@googlegroups.com
use water with Chloride content less than
 25 ppm
use potable water
do water analysis 

On Fri, 18 Sep 2020, 15:38 Manish Kumar, <mkmk...@gmail.com> wrote:
Dear Sir,
I want to know that which type of water is used for Hydrotest in stainless steel piping and equipment. Please advise as per relevant code and standard.




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHfQ4k7ZV%2B%3DrkXu%3DSdnx2zeGsMf83xjjA%2B4-CLvDzZ1TBuuBfg%40mail.gmail.com.

Manish Kumar

unread,
Sep 18, 2020, 8:18:50 AM9/18/20
to material...@googlegroups.com
Sir,
How much Ph value is required for Hydrotest in Stainless steel piping and equipment.Please advise as per reference of relevant standard & Code.

Prakash Hegde

unread,
Sep 18, 2020, 10:55:23 AM9/18/20
to material...@googlegroups.com
Hi!
It should be.less than 25 ppm
It also depends upon service application of.eqpt.and concern spec
Generally.kept below 25ppm
Regards

Dhaneesh p

unread,
Sep 18, 2020, 10:55:23 AM9/18/20
to material...@googlegroups.com
Dear , 
As follow saudi aramco standard and procedure ,  saes-a-004, saes-l-150, following are my observations

Water used for hydro testing of stainless steel piping systems shall have chloride content value less than 50ppm, and PH value should be 7.5, ±.5.

Water used for any part of the hydro testing or subsequent lay-up shall have a sulfate reducing bacteria (SRB) count of 10³ per ml or less

When the equipment contact time with hydrotest water may exceed 14 days, an approved oxygen scavenger shall be added to the hydrostatic test water.

For stainless-steel piping, the duration of the hydro testing (using water with less than 50 ppm of chlorides), flushing and draining-drying sequence shall be kept as short as possible, in order to reduce the possibility of chloride attack. Water testing certificate will be made available for each hydro test

regards 

Dhaneesh 



George Dilintas

unread,
Sep 23, 2020, 9:36:08 AM9/23/20
to material...@googlegroups.com
Codes does not specify water quality

Στις Παρ, 18 Σεπ 2020 στις 2:38 μ.μ., ο/η Manish Kumar <mkmk...@gmail.com> έγραψε:
Dear Sir,
I want to know that which type of water is used for Hydrotest in stainless steel piping and equipment. Please advise as per relevant code and standard.




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHfQ4k7ZV%2B%3DrkXu%3DSdnx2zeGsMf83xjjA%2B4-CLvDzZ1TBuuBfg%40mail.gmail.com.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics