Try a slower welding speed and a closer arc length.
Regards, 9 4 2020.
David Harvey
Thanks & Regards
J.Gerald Jayakumar
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1877339917.2035801.1586429580458%40mail.yahoo.com.
--
- check the hardness of BM away from welding and what Is the welding HV values ?- HAZ prosperities mainly related to the base metal- your base metal SA516 in normalised condition .. after welding the mech. priorities gained by heat treatment is lost unless u keeping the transformation temp. and cooling rate as the original treatment condition- any way .. as much as u can try to increase HI for getting the lowest cooling ratebest regards
Guys i am developing weld procedures for automated orbital welding and having trouble trouble with achieving required hardness.--SA-516-70N 2"Thk tube sheet / SA-179 1"OD x 6"Lg Tubes different wall thickness. Preheating 400 interpass 600 FI am having isues with hardness on the heat affected zone. The criteria to meet is 248 Hv10 (vickers). Especially at the Haz zone iam getting 300 vickers.Anyone have experience in tube to tube sheet welding can offer some suggestions that will be great.My best results were in 0.095 wall thickness where HAZ readings were close to 250 still failed becauseit was marginally over. 0.065, 0.83 failed with HAZ hardness averaging at 300.Best reagrdsTesh
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
Problems related to Hardness may be due to High Heat Input or preheat being applied not properly (temperature is OK) you may look at the option of reducing the cooling rate or checking at the Carbon EquivalentThanks & Regards
J.Gerald Jayakumar
On Thursday, April 9, 2020, 05:31:05 PM GMT+7, 'd...@btinternet.com' via Materials & Welding <material...@googlegroups.com> wrote:
Try a slower welding speed and a closer arc length.
Regards, 9 4 2020.
David Harvey
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
To view this discussion on the web visit
- check the hardness of BM away from welding and what Is the welding HV values ?- HAZ prosperities mainly related to the base metal- your base metal SA516 in normalised condition .. after welding the mech. priorities gained by heat treatment is lost unless u keeping the transformation temp. and cooling rate as the original treatment condition- any way .. as much as u can try to increase HI for getting the lowest cooling ratebest regards
Guys i am developing weld procedures for automated orbital welding and having trouble trouble with achieving required hardness.--SA-516-70N 2"Thk tube sheet / SA-179 1"OD x 6"Lg Tubes different wall thickness. Preheating 400 interpass 600 FI am having isues with hardness on the heat affected zone. The criteria to meet is 248 Hv10 (vickers). Especially at the Haz zone iam getting 300 vickers.Anyone have experience in tube to tube sheet welding can offer some suggestions that will be great.My best results were in 0.095 wall thickness where HAZ readings were close to 250 still failed becauseit was marginally over. 0.065, 0.83 failed with HAZ hardness averaging at 300.Best reagrdsTesh
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
Higher hardness could mean:Higher residual stressesMartensite formationThe most probable cause are Higher residual stresses.To reduce the residual stresses are following options:1. Increase preheat. You may try 100degC2. Decrease interpass temperature. You May try 150 degC3. Decrease heat Input by shortening the arc or Increase welding spead
Στις Πέμ, 9 Απρ 2020, 13:31 ο χρήστης 'd...@btinternet.com' via Materials & Welding <material...@googlegroups.com> έγραψε:
--
Try a slower welding speed and a closer arc length.
Regards, 9 4 2020.
David Harvey
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b64cfe46-db32-4110-b3ae-74f21cd0670d%40googlegroups.com.