Procedure qualification through AWS

270 views
Skip to first unread message

praba karan

unread,
Mar 2, 2026, 4:26:27 AMMar 2
to Materials & Welding
Dear experts,

For procedure qualification as per ASME SEC IX- "Multiple PQRs may support one WPS",

Likewise can we follow the same practice in AWS also?  Because which is not mentioned directly on the code that we can use multiple PQRs to support one WPS.(And I'm not using prequalified WPS)


Thanks & regards
Prabaharan

Sajeersayed Ali

unread,
Mar 2, 2026, 4:39:06 AMMar 2
to material...@googlegroups.com
5.2.2 Combination of WPSs. A combination of qualified and prequalified WPSs may be used without qualification
of the combination, provided the limitation of essential variables applicable to each process is observed.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/f0bb15a1-0ff5-4d62-b662-1b365472aadbn%40googlegroups.com.

james gerald

unread,
Mar 2, 2026, 5:36:44 AMMar 2
to material...@googlegroups.com
I suppose you can support only for welding positions.

Unlike ASME Sec.IX code for process vessels & piping where the Load is uniform and the materials are restricted by code it allows for combination.

But AWS D 1.1, you are subjected to Static, Dynamic & cyclic loading as well and as such there is no statement like ASME Sec.IX like combining WPS/PQR. Moreover you prepare WPS for 1 Pressure vessel and it is easy to control in the shop but whereas AWS D1.1 say for example offshore platforms, you have many varied components like Beam, Plates, girders, tubulars etc.. and it is difficult to control. Only for need based WPS to be used for AWS D1.1.

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635



--

james gerald

unread,
Mar 2, 2026, 5:41:58 AMMar 2
to 'james gerald' via Materials & Welding
Just to add, Pressure vessels is designed mostly for Internal pressure & external pressure.

section 5.2.2 is for combination of qualified & prequalified WPS and not pertaining PQR's.

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635

sridhar cn

unread,
Mar 2, 2026, 12:03:49 PMMar 2
to material...@googlegroups.com

AWS D1.1 does not restrict the number of PQRs supporting a WPS. Clause 6 requires only that essential variables be validated by procedure 

qualification testing. Where a single PQR does not cover all required variables of a production WPS, multiple PQRs may be combined to provide 

full technical support. Therefore, using multiple PQRs to support one WPS is fully acceptable and code-compliant. 

Sridhar.


Md Usman Ghani

unread,
Mar 17, 2026, 6:09:21 AMMar 17
to material...@googlegroups.com
Just for clarification
Can any one share, WPS, for ss410 to SS316,

sridhar cn

unread,
Mar 17, 2026, 11:35:33 AMMar 17
to material...@googlegroups.com

Giving below are the hints for WPS (both ISO / AWS) for joining SS 410 (martensite) to SS 316 (austenitic). 

This should be supported by a PQR qualification. 

WPS: Dissimilar Joint: SS 410 vs. SS 316 

1. General Information:

Process: GTAW (Root) + SMAW / GMAW (Fill & Cap); Type: Dissimilar stainless steel welding

2. Base Materials:

SS 410 (UNS S41000) – 410 Martensite SS to  SS 316 – Austenitic SS; ASME sec. IX P no 6 (410) to Pno 8 (316)

3. Joint Details:

Joint Type: Butt joint;  Thickness Range (Qualified): xx mm – xx mm (based on the PQR)

Root Gap: 2–3 mm; Bevel Angle: 60° included; Backing: Optional (SS backing or GTAW root) 

4. Filler Metal:

Primary Choice: ER309L / E309L (for welding);  Alternative (for critical service): ERNiCr-3 (Inconel 82)

GTAW: ER 309L / ER NiCr-3; SMAW: E 309L / ENiCrFe-3; GMAW: ER309L

(309L acts as a buffer to handle dilution & prevent cracking; Ni-base reduces risk of martensite cracking)

5. Welding Parameters: GTAW (root) Polarity: DCEN ; Shielding gas: Argon (99.99%) Flow rate: 10–15 L/min

SMAW (fill/cap).Polarity: DCEP; GMAW (Optional) Mode: Spray / Pulse; Gas: Ar + 2–5% CO₂ or Ar + 2% O₂ 

6.Preheat & Inter-pass Temperature: Preheat  200-300 degC (for SS 410 to avoid cracking); Inter-pass 250 deg.C. 

7. PWHT (for SS 410): SR at 650-700 deg C; Holding time- 1hr / 25 mm thick; Cooling- Controlled furnace cooling. 

8. Special Technique: Buttering recommended on SS 410 side with ER309L to void cracking; Stringer beads preferred (no weaving)

9. Inspection & Testing: 100% VT+ PT + RT / UT – As per the requirement;  Hardness check (important on 410 side & HAZ) 

Trust above details will help you to prepare your WPS & PQR.

 

Sridhar.

-------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


Sankaran Sp

unread,
Apr 29, 2026, 3:08:50 AMApr 29
to material...@googlegroups.com
Dear Mr Sridhar,

good & wishes for detailed explanation for welding of dissimilar material . All the inputs & parameters are found as good and meeting the standard requirements. small suggestion on PWHT temperature as given below:
as per ASME sec VIII div-1 for 410 type steel- PWHT temperature will be 760deg C, kindly check & proceed further       

Regards,
Sankaran.SP
Welding & Metallurgy expert
Coimbatore, India. 


sridhar cn

unread,
Apr 29, 2026, 11:23:11 AMApr 29
to material...@googlegroups.com

 Dear Mr. Sankaran,

1.  For SS 410 (martensitic stainless steel), PWHT directly affects hardness, toughness, and risk of cracking. Metallurgically SS 410 forms untempered 

     martensite after welding, so PWHT is mandatory in most cases. PWHT is required to temper martensite, reduce hardness, and relieve residual stresses.

2.  Applicable Standards / References: ASME Section II / IX – Material & Welding Qualification. AWS D1.6 – Structural Welding Code (Stainless Steel); 

     Industry practice for martensitic (410/420 series) SS materials.

3.  Evaluation of PWHT Temperature Options:

   Option 1: 650–700°C (Selected range)- Achieves effective tempering of martensite. Reduces hardness to acceptable range (~200–250 HV). Maintains 

     optimum balance of strength and toughness. Minimizes risk of over-tempering, grain coarsening and loss of mechanical properties.

   Conclusion: Metallurgically stable and widely accepted range for SS 410.

   Option 2: ~760°C (Higher range) - Produces further softening (lower hardness), may improve ductility marginally, however it introduces risks of over-

     tempering resulting in reduction in tensile strength, possible degradation of creep/structural properties. This typically used when hardness reduction is 

     critical (e.g., NACE/ field service requirement), when the weld is too hard (>~250–275 HV), and for thick restrained joints. Not required unless hardness 

     reduction is specifically mandated and service conditions demand higher ductility. 

     Conclusion: Not preferred for general applications. 

4.  Code Compliance: ASME and AWS do not mandate a fixed PWHT temperature for SS 410. They require a PQR demonstrating acceptable properties, 

     control of hardness, strength, and soundness. The selected range 650–700°C complies, as it produces acceptable mechanical properties during qualification.

5.  Justification: The PWHT temperature range of 650–700°C is selected because, It ensures adequate tempering of martensitic structure; Achieves required 

     hardness  reduction  without compromising strength; Avoids risks associated with higher temperature exposure (~760°C); Aligns with established industry 

     practice and metallurgical principles. Meets procedure qualification and code acceptance criteria. 

6.  Conclusion: PWHT at 650–700°C (1 hr/25 mm, furnace cooling) is technically justified, code-compliant, and optimal for SS 410 weldments. PWHT at ~760°C   

     is not necessary and is only to be used when specifically required by design or hardness criteria. 

7. The choice: Depends upon the field requirements.

 

Sridhar.

------------------------------------------------------------------------------------------------------------------------------------------------


Vishwas Keskar

unread,
May 1, 2026, 10:47:08 PMMay 1
to material...@googlegroups.com
What is thickness ?
Pl check use of TYP410 S 
This Will possible that you will epsilon ate PWHT as I can see typ316  is there on other side .
Pl speak to Engineering Team and discuss further 
for service conditions of the joint being used .
Vishwas 
IWE
9823472273
India 

Sankaran Sp

unread,
May 2, 2026, 5:21:07 AMMay 2
to material...@googlegroups.com
Dear Mr Sridhar,

Thanks a lot for your valid reply with acceptable reasons, very nice explanation. good & appreciate your effort.   

Regards,
Sankaran.SP
Welding & Metallurgy expert

Ashishranjan - Domech Fabricators Pvt.Ltd.

unread,
May 4, 2026, 5:48:44 AMMay 4
to material...@googlegroups.com
Yes, you can use multiple PQRs to support a single WPS under AWS as well but it’s handled a bit differently than in ASME Section IX, and you need to be careful about how you justify it.
  

Regards,

Ashish Ranjan

+91 9555864374

Go green logo

Save a tree...Please consider your environmental responsibility. Before printing this e-mail message, ask yourself whether you really need a hardcopy.



"Confidentiality Warning: This message and any attachments are intended only for the use of the intended recipient(s), are confidential and may be privileged. If you are not the intended recipient, you are hereby notified that any review, re-transmission, conversion to hard copy, copying, circulation or other use of this message and any attachments is strictly prohibited. If you are not the intended recipient, please notify the sender immediately by return email and delete this message and any attachments from your system.

Virus Warning: Although the company has taken reasonable precautions to ensure no viruses are present in this email. The company cannot accept responsibility for any loss or damage arising from the use of this email or attachment."


Caution: The e-mail below is from an external source. Please do not open attachments or click links unless this email comes from a known sender and you know the content is safe.



--

sridhar cn

unread,
May 5, 2026, 5:45:04 AMMay 5
to material...@googlegroups.com
Dear Mr. Sankaran,
Thanks for the reply and your understanding.
rgds,
Sridhar.

Kannayeram Gnanapandithan

unread,
May 8, 2026, 12:28:59 AMMay 8
to material...@googlegroups.com
could pl  share the reference where it is given
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 1090 & EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


sridhar cn

unread,
May 8, 2026, 11:15:47 AMMay 8
to material...@googlegroups.com
From the available Technical literatures.
CS.

manish kulkarni

unread,
May 8, 2026, 12:44:13 PMMay 8
to material...@googlegroups.com
Hi respected group members,

Pl share some experience on weld overlay on F6Nm material?

sridhar cn

unread,
May 11, 2026, 8:04:24 AMMay 11
to material...@googlegroups.com

 Though I have not done actual overlay, what I could gather from the available literature is that, F6NM Stainless Steel weld overlay is 

 commonly  done in hydro turbine parts, valve internals, and pump sleeves . The success of overlay depends much more on dilution control, 

 hydrogen control, and post-weld hardness management than on the actual deposition process itself.

 F6NM / CA6NM is a P6, air hardening low carbon martensitic stainless steel with approx. 13% Cr + 4% Ni + 1% Mo. Its UTS is 750-950 MPa,                                   Yield  550-750 MPa, 15-22% EL and hardness 259-320 HB. Major issues observed during overlay are: Underbead cracking; delayed hydrogen 

cracking; toe cracking after 24–72 hrs; hard martensitic HAZ overlay disbonding during service.This happens because F6NM transforms to 

untempered martensite very easily during cooling.Typical HAZ hardness without proper control would be 420–550 HV and highly crack-sensitive.

To avoid them, a  mandatory preheat at 150–250°C and an inter pass temperature of 180–250°C to be maintained. Low heat input should be  

avoided as  it causes fast cooling and forms martensite structure. Typical heat input range could be 1.5-2.0 kJ/mm. Excessive high heat input 

may create Ferrite in-balance. Final overlay (Stellite, Ni alloy 625 or SS)  should be done after buttering with ER 309L  to avoid martensitic cracking;  

PWHT at 580–620°C (furnace cooled up to 300 Deg C) for 2–4 hrs or controlled welding with preheat + slow cooling is recommended to improve 

toughness. Usually a 2- layer minimum deposit is done; First layer may have high dilution and the second or third layer will have required chemistry.

Low hydrogen consumables, dry shielding gas, and clean surface are required to avoid Hydrogen (due to moisture/contamination) are mandatory. 

Preferred furnace cooling or insulation blanket cover to avoid fast cooling. Recommended hardness targets are HAZ < 350 HV; Overlay transition 

< 380 HV; Higher values usually indicate cracking risk.

For restrained and heavy F6NM components, no direct deposit on the cold base metal should be done. Never stop welding midway and leave partially   

heated components overnight. Maintain minimum holding temperature until welding completion.  A large number of failures originate from thermal 

cycling interruptions.

Trust above info. may be of help to you. 

C Sridhar.

----------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


manish kulkarni

unread,
May 11, 2026, 1:02:56 PMMay 11
to material...@googlegroups.com
Yes, literature is available, but looking for actual production experience as normally martensitic SS.  , weld overlay is not performed. 

sridhar cn

unread,
May 12, 2026, 4:37:28 AMMay 12
to material...@googlegroups.com
What problems are you expecting to face during pre and post overlay welding operations? 
You have not yet spelled out whether it will be Stellite, Ni based or SS based overlay and
on what thickness? 
Could mention only the expected problems and precautions /solutions to avoid them in advance. 
Unless the actual welding (PQR) is done, we will not know what practical problems to face. 
Think you can guide us with your experience.
All the Best!!
rgds,

manish kulkarni

unread,
May 12, 2026, 7:42:59 AMMay 12
to material...@googlegroups.com
We are qualifying PQrs for 625 WO on F6 Nm.   I foresee risk due to micro structure changes due to higher PWHt temp against tempering temp of C6 Nm . 
Also checking hardness control for cracking in HAZ as service is very high sour and high pressure. 
So if anybody has qualified PQR , was checking on above parameters. 
Thanks , 

luis carlos greggianin

unread,
May 12, 2026, 12:27:48 PMMay 12
to material...@googlegroups.com
pré-heating: 150-200ºC
ER410
optional Pós heating: 300ºC/1 h

james gerald

unread,
May 12, 2026, 10:14:02 PMMay 12
to material...@googlegroups.com
Preheat substrate  base material to 150-260degC.
Use 309L or 309LMo as barrier layer or buffer layer for 1-2 passes.
Apply E410 for better corrosion resistance.
Perform Tempering on the weld

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635

james gerald

unread,
May 12, 2026, 10:14:02 PMMay 12
to 'manish kulkarni' via Materials & Welding
1. Use Preheat of 150degC to 250degC. Higher preheat temperature may result in retained Austenite and also upon overlay cool it to Room temperature or temperature below the Mf (Martensite finish temperature).
2. Use ER/ENiCrMo3 for the barrier layer as well as remaining passes.
3. Perform PWHT at least 30degC below the Material tempering temperature to avoid softening due to coarsening of carbides or pearlite spherodization.
4. Post heat at 300degC after welding may be beneficial to drive away Hydrogen.

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635

Bhavani Prasad Emani

unread,
May 13, 2026, 6:12:51 AMMay 13
to 'manish kulkarni' via Materials & Welding
Hi Manish,

Here are some considerations and insights

ParameterRecommendation
Preheat150–250°C (300–480°F) 
Interpass TemperatureMax 250–300°C (480–570°F)
PWHT (Post-Weld Heat Treatment)Required for sour service, toughness restoration 
PWHT Temperature595–650°C (1100–1200°F), then slow cool 
Mechanical PeeningAvoid (causes martensite transformation, increases hardness)
Hardness ControlMaintain ≤23 HRC after PWHT for NACE compliance 
Filler Metal (repair/matching)ER410NiMo (AWS A5.9) or E410NiMo (AWS A5.4) – matches F6NM composition 
Filler Metal (corrosion overlay)ER309L (first pass) + ER316L (final pass) or ERNiCr-3/Inconel 625 for superior CRA 

IssueSolution/Best Practice
Cracking riskF6NM is air-hardening; preheat 150–250°C mandatory 
HAZ hardeningUse low heat input + controlled interpass temperature 
PWHT requirementAlways do PWHT after welding F6NM for sour service or critical applications 
Hardness超标After PWHT, check hardness ≤23 HRC (NACE MR0175) 
Overlay composition verificationMandatory PMI on overlay (especially final pass chemistry) 
Microstructure checkVerify no excessive martensite in HAZ, proper tempering after PWHT 
Grind flush before overlayRemove surface defects, scale, contaminants from F6NM before overlay 
DPI/PT testingPerform PT after each pass and after final overlay for defects 


Thanking you,

With best regards,                                            
           
Bhavani Prasad Emani,



manish kulkarni

unread,
May 13, 2026, 7:27:17 AMMay 13
to material...@googlegroups.com
Guys 
Complete weld overlay , no butt weld.   Anyway thx.  We have completed the activity 

Regards 

james gerald

unread,
May 13, 2026, 8:27:32 AMMay 13
to 'manish kulkarni' via Materials & Welding
Either clad restoration weld overlay or weld overlay for the entire vessel or piping, technical points remain the same.

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635

sridhar cn

unread,
May 14, 2026, 1:34:36 PMMay 14
to material...@googlegroups.com
Nice, if so, Please share the results.

Final thoughts from my end:

F6NM is an air-hardening steel. During welding Austenite forms and transforms into fresh Martensite which is a hard, brittle and crack sensitive 

leading to delayed cracking.Typical as-welded HAZ will have a coarse-grained HAZ with a hardness of 400–550 HV. Any moisture picked through contamination/migration turns into hard martensite and causes delayed Hydrogen cracking after 24–72 hrs.

Hence, Preheating at 150–250°C (very important) and an inter pass temperature of 180–250°C reduces cooling rate, avoids thermal stresses  

and provides lower hardness and lower crack susceptibility. Butter layer with ER 309L (Austenite absorbs stresses better, hydrogen solubility higher;                  cracking resistance improves) provides metallurgical cushion layer and will help to reduce the dilution and corrosion resistance.

The PWHT temp at 580–620°C (furnace cooled up to 300 deg C) for 2–4 hrs tempers fresh martensite, relieves stress; precipitate fine carbides.                                       Any excessive over-tempering occurs; strength drops toughness may deteriorate.  For a successful F6NM overlay, Keep the HAZ soft enough.

Sridhar.                                    .