Dear Members,

I would like to know difference between IS 1367 Gr. 4.6, 8.8 & 10.9
What does "4.6", 8.8 and "10.9" means....... 

Thankyou

V. B.

Vino Varghese

unread,
Dec 8, 2012, 3:32:59 AM12/8/12
to material...@googlegroups.com
Dear Baskar,

It differ in tensile and yield strength of Fastener material. 
Browse the internet and you will find this basic difference.

Regards
Vino-Doha


V. B.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Muthusrinivasan Muthuselvam

unread,
Dec 8, 2012, 1:08:45 AM12/8/12
to material...@googlegroups.com
Dear Mr.V.B,
 
for exaple 4.6 means---> first digit 4 refers nominal UTS in hundreds ie., 400 N/sq.mm , second digit .6 means  lower yield stress in tens ie., 60 N/sq.mm
 
br,
 
msms 


V. B.

--

Shivashankrappa Balawat

unread,
Dec 7, 2012, 6:45:19 AM12/7/12
to material...@googlegroups.com

Mr.Bhaskar,

 

This is fastener standard for bolts

Grade 8.8 means , Approx. 800 MPa TS and 640 MPa yield strength(  you will arrive at the YS by multiplying the both the numbers times 10. That is 8x8x10=640)

Similarly  , 10.9 means  approx.1000 MPa  TS and 900 MPa yield strength. I have given below the exact details.

 

 

Property Class

Tensile strength,Mpa

Hardness

Material

heat treatment

tempering

4.6

400

B67-B87

low or medium carbon steel witth max limits for C 0.55, P0.048, S0.058

no

 

4.8

420

B71-B87

5.8

520

B82-B95

8.8

830

C23-C34

 medium carbon steel with max limits for C0.28- 0.55, P0.048, S0.058

oil quenched

 min 425 deg C

9.8

900

C27-C36

 min 410 deg C

10.9

1040

C33-C39

 min425  deg C

12.9

1220

C38-C44

 medium carbon steel with max limits for C0.31- 0.65, P 0.045 MAX, S 0.045MAX

oil quenched

min 380deg C

 

I hope this will clarify your point. If any questions please don’t hesitate to write.

 

Regards,

 

S C Balawat.

--

Ravishankar G

unread,
Feb 10, 2016, 4:05:54 AM2/10/16
to Materials & Welding
Is there any relation to RC or Brinell Harndess to that of the class???

amol gengaje

unread,
Feb 18, 2016, 10:47:47 PM2/18/16
to material...@googlegroups.com

In 4.6 ,4 means 40kg/mm2 tensile & 6 means 0.6 of 40 I.e.24 kg/mm2 yield.similar for other classes.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/37f21378-624e-4b12-93b6-2cbb7da3049f%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Ajith Kumar

unread,
Jul 19, 2016, 12:12:02 PM7/19/16
to Materials & Welding
Hello, This information is very usefull.

Currently I have a requirement to produce M8 --8.8 grade Bolt. 
Can I select material C40 for the same.

Ajith

Alan Denney

unread,
Jul 21, 2016, 4:26:08 AM7/21/16
to material...@googlegroups.com

To the moderator

 

I am disappointed that my mildly worded expression of concern has not been released by you. The original author appears to have little understanding of the subject of high tensile bolts and this merits comment, when lives may be at risk from the product manufactured by that correspondent.

 

Alan

 

Alan Denney

AKD Materials Consulting Ltd

 

From: Alan Denney [mailto:al...@denney1.freeserve.co.uk]
Sent: 19 July 2016 19:45
To: 'material...@googlegroups.com' <material...@googlegroups.com>
Subject: RE: 25120] Re: 16160] Difference between IS 1367 Gr. 4.6, 8.8 & 10.9

 

I am surprised. You appear to be about to make high tensile bolts, but do not understand the grade designation and are asking others to do your material selection for you, and without mentioning the diameter of the bolt which is a critical factor in getting the properties. Making bolts which are fit for service requires in-depth understanding of all aspects of the job.

                                                                                                                                

Alan Denney

AKD Materials Consulting Ltd

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

---

You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.


For more options, visit https://groups.google.com/d/optout.

 

This email has been scanned by BullGuard antivirus protection.

For more info visit www.bullguard.com


This email has been scanned by BullGuard antivirus protection.
For more info visit www.bullguard.com

Alan Denney

unread,
Jul 21, 2016, 4:26:37 AM7/21/16
to material...@googlegroups.com

I am surprised. You appear to be about to make high tensile bolts, but do not understand the grade designation and are asking others to do your material selection for you, and without mentioning the diameter of the bolt which is a critical factor in getting the properties. Making bolts which are fit for service requires in-depth understanding of all aspects of the job.

                                                                                                                                

Alan Denney

AKD Materials Consulting Ltd

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Ajith Kumar


Sent: 19 July 2016 07:27
To: Materials & Welding <material...@googlegroups.com>

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/446d60dc-1874-4d29-8cb2-54ecaac10e2a%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Reply all
Reply to author
Forward
0 new messages