Greetings,
Need expert opinion for the following query:
Construction Code ASME B31.3, Qualification ASME BPV Sec. IX.
One of the WPS is qualified for Low temperature Carbon steel with impact testing and PWHT. The qualification range is 20mm to 36mm. 
PWHT is applicable (Project specification). Soaking time was 1 hr 30 minutes.
Question: Is this WPS qualified for a repair weld with this soaking time? 
Is a new PQR to qualify the repair joint?

Best Regards,

cid:image001.png@01D0FB95.19500D80

Muhammad Babur Khan Lashari
Project Quality Supervisor.
API 570, API 510, CSWIP 3.2.2. ISO 9001:2015

Mob: +966 58 2774568 / +966 51 0559680

Please consider the environment before printing this e-mail

Sampath Kumar

unread,
Jan 27, 2026, 9:49:48 PMJan 27
to material...@googlegroups.com
Greetings 

Yes — only if the repair weld falls entirely within the qualified range and the PWHT performed meets the same essential variables as originally qualified.
If any variable in the repair (thickness, PWHT hold time, PWHT temperature, base material, filler metal, joint design) exceeds the qualified range, then the existing WPS cannot be used and a new PQR is required.
Best regards


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAN53wK16%2Bvf43xPRxmXync%3DGa42jqR7kk70ou7vyCdT9MShcZQ%40mail.gmail.com.

Anandhapadmanabha pillaim

unread,
Jan 27, 2026, 9:49:49 PMJan 27
to material...@googlegroups.com
The qualification range would be 16 to 36mm if you qualify a PQR On 18mm plate thickness, PWHT soaking on pqr is 1hr 30mins so maximum soaking with impact will be 1hr 52.5hrs, if you are doing the resoaking and if the total soaking time ( Actual PWHT & Repair PWHT soaking time) is within this range you can use this, if it exceeded need to requalify.

The above explanation is based on With impact testing below the Lower transformation temperature (AC3)

--

ananth karuppanan

unread,
Jan 27, 2026, 9:49:49 PMJan 27
to material...@googlegroups.com
Dear 

New PQR need to be qualified for the repair welding as per the client requirements.

Thanks & Regards,
Ananth Karuppanan.
               +971-588925593


--

Anandhapadmanabha pillaim

unread,
Jan 27, 2026, 10:07:37 PMJan 27
to material...@googlegroups.com
If new PQR qualification as per client specification is there means no need to ask this question, normal & repair PQR should be qualified separately. If we are talking on the basis of ASME SEC 9 & ASME B31. 3, below Explanation is sufficient.


The qualification range would be 16 to 36mm if you qualify a PQR On 18mm plate thickness, PWHT soaking on pqr is 1hr 30mins so maximum soaking with impact will be 1hr 52.5mins, if you are doing the resoaking and if the total soaking time ( Actual PWHT & Repair PWHT soaking time) is within this range you can use this, if it exceeded need to requalify.

The above explanation is based on With impact testing & PWHT below the Lower transformation temperature (AC3)

james gerald

unread,
Jan 28, 2026, 12:48:15 AMJan 28
to material...@googlegroups.com
See snap shot below from ASME B31.3. No Repair procedure is required. But PWHT has to be performed after Repair. PWHT soaking time should have been added during the original PQR Qualification or Simulated test coupon including Repair soak time shall be included during Material testing.


Inline image

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635



--

Babur Khan

unread,
Jan 28, 2026, 10:22:41 PMJan 28
to material...@googlegroups.com, material...@googlegroups.com
Greetings,
Thank you for your kind response.
In pur PQR, soaking time for repairs Welding not considered. 

Muhammad Babur Khan
Sent from my iPhone

On 28 Jan 2026, at 8:48 AM, 'james gerald' via Materials & Welding <material...@googlegroups.com> wrote:


See snap shot below from ASME B31.3. No Repair procedure is required. But PWHT has to be performed after Repair. PWHT soaking time should have been added during the original PQR Qualification or Simulated test coupon including Repair soak time shall be included during Material testing.


<1769579047580blob.jpg>


Thanks & Regards

J.Gerald Jayakumar

0091-8838619635

On Wednesday, 28 January 2026 at 07:48:56 am IST, Babur Khan <mbabu...@gmail.com> wrote:


Greetings,
Need expert opinion for the following query:
Construction Code ASME B31.3, Qualification ASME BPV Sec. IX.
One of the WPS is qualified for Low temperature Carbon steel with impact testing and PWHT. The qualification range is 20mm to 36mm. 
PWHT is applicable (Project specification). Soaking time was 1 hr 30 minutes.
Question: Is this WPS qualified for a repair weld with this soaking time? 
Is a new PQR to qualify the repair joint?

Best Regards,

<image001.jpg>

Muhammad Babur Khan Lashari
Project Quality Supervisor.
API 570, API 510, CSWIP 3.2.2. ISO 9001:2015

Mob: +966 58 2774568 / +966 51 0559680

Please consider the environment before printing this e-mail

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAN53wK16%2Bvf43xPRxmXync%3DGa42jqR7kk70ou7vyCdT9MShcZQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/411193529.3005035.1769579048563%40mail.yahoo.com.
<1769579047580blob.jpg>
<image001.jpg>

james gerald

unread,
Jan 29, 2026, 5:42:06 AMJan 29
to material...@googlegroups.com
 ASME B31.3 refers ASME Sec.IX for WPS/PQR qualification. PWHT Soak time after Repair will be considered during original PQR qualification and when Charpy Impact tests are required, below snap shot of ASME Sec.IX applies.

Inline image
Normally in Pipe Mill, MPQ (Manufacturer Procedure Qualification) with welding & Heat Treatment will be performed including repair PWHT cycles during pipe production.

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635