[MW:5177] PQR tests for tube to tube-sheet strength weld joint -- ASME Sec.VIII div.1

2,070 views
Skip to first unread message

pgos...@sympatico.ca

unread,
May 14, 2010, 4:38:18 PM5/14/10
to material...@googlegroups.com



Dear Fede,

 

Please look at ASME Sec-VIII, DIV-1, Non-Mandatory Appendix A, Basis for Establishing Allowable Loads For Tube To-Tube-sheet Joints.

Para A-3 Shear Load Test, details out the tear test and how it’s to be performed. This test is commonly dubbed as Pull-Out Test by many specifications.

 

Tube –tube sheet qualification test, shall be done as per ASME Sec-IX-QW -193. Sec-IX calls for Visual, LPI and Macro examination. Tear test is normally over and above ASME requirements.

 

For you case the testing on PQR should be ASME Sec-IX, Visual, LPI and Macro examination + Tear Test/Pullout test. Pull out test would require a separate  tube to tube sheet welding block.

Hope it clarifies your  query.

                                                                                                                                                                                                                                                        

 

Pradip Goswami, P.Eng.

Welding /Metallurgical Engineer-Specialist

Email-p...@sympatico.ca, pgos...@quickclic.net.  

 

 


Date: Fri, 14 May 2010 19:54:57 +0400
Subject: Re: [MW:5174] PQR tests for tube to tube-sheet strength weld joint - ASME sez.VIII div.1
From: atulcha...@gmail.com
To: material...@googlegroups.com

you have to follow TEMA for heat exchanger and accordingly do the Pull-out

test.

 

 

 

On Wed, May 12, 2010 at 1:35 AM, federico.29 <feder...@fastwebnet.it> wrote:

Dear sirs,
according to ASME sec .VIII div.1, which tests are required to perform in PQR for a tube to tube-sheet strength weld joint? in particular tear test is required? (please give me the reference of para of ASME sec.VIII div.1), material involved is Carbon Steel: A350 (tube-sheet) and A334 (tube) welding process is GTAW machine thickness involved: 70 mm (tube-sheet) and 2.77 mm (tube)
Thank in advance
Fede Lau

--

To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Reply all
Reply to author
Forward
0 new messages