need to clarify some sentences in the AWS D1.1 2025 edition

26 views
Skip to first unread message

krishna magdum

unread,
Aug 20, 2025, 9:04:07 AMAug 20
to material...@googlegroups.com

Dear Sir,
I need to clarify some sentences  in the AWS D1.1 2025 edition
1. table 6.6   PQR essential variable changes.. for voltage > 07 %, current  >10% increase or decrease......if  PQR qualified range 26 to 28 V and 170 to 180 A  then how much value we can keep for min to max for range qualification, either consider higher side value or lower side value

2. For CVN test min thick qualification 12 mm to unlimited  for 25 mm thick weld coupon plate but  we need below 12 mm plate thick qualification we have taken 06 mm weld coupon plate thick. but standard mentioned... minimum thickness qualification 03 mm 
 we need 03 mm thick ness to unlimited thickness QUALIFICATION what should do..
  a)  either required two weld coupons 25 mm and 06 mm thickness those 25 mm weld coupons complete the limite 12 mm to unlimited and 06 mm weld coupons complete the limite 2T that is 03 mm to 12 mm Thick....

Please clear this concern..

image.png


image.png



               Thanks You

        

          Mr. Krishna Magdum

          




Please be environmentally friendly. Print this email, if you actually need it.

 

  

    







 

Anandhapadmanabha pillaim

unread,
Aug 20, 2025, 9:45:38 AMAug 20
to material...@googlegroups.com
Below information is for your clarification,

If you qualify with  26- 28 voltage the range of qualification for voltage is 24.18 - 29.96V and Current 153A - 198A.
For CVN for 25mm range of qualification is 12 to unlimited. For 6mm range of qualification is 6mm to 12mm. Inorder to cover from 3mm, We need weld one coupon whose thickness is less than 6mm then (Eg: 5.9) it will cover from 3 mm to 11.8mm.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CANV5kQ6WBCrVNPnU42Zxrf3Y5hBA-sHEz2g2UM_czQnGFinihw%40mail.gmail.com.

krishna magdum

unread,
Aug 21, 2025, 2:04:57 PMAug 21
to material...@googlegroups.com


Dear Sir,
Thanks you so much for your reply...
 Similar I need range for
1)  travel speed, 160 to 170 mm / min.
 >10%  increase or decrease 
2) wire feed speed mtr/min... 1.3