Ponnikumar

unread,
Nov 29, 2022, 5:25:29 AM11/29/22
to material...@googlegroups.com
Dear gentlemen,
My client inspector told me to do button weld test on plate for filler wire 309L . The dimension are follow as asme sec II c then need to do PMI verification 

My query is any requirements by code for filler wire button test for all filler and electrode and why it required ? 



Faisal Quadri

unread,
Nov 29, 2022, 6:05:47 AM11/29/22
to material...@googlegroups.com
SAES A 206  Aramco requirement 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKL%3DdYw73OyFYLq4yTHUB2cVqbuaDCCunxc73%2BaU0kJZurJd%2Bw%40mail.gmail.com.

Ponnikumar

unread,
Nov 29, 2022, 10:17:18 PM11/29/22
to material...@googlegroups.com
Hi sir,
Except Aramco standard. Can you explain from ASME codes 

Mostafa Kamel

unread,
Nov 29, 2022, 10:17:19 PM11/29/22
to material...@googlegroups.com
Hi
There are NO code requirements for button weld test. Kindly review project specification or ask the client the reason for the button weld test. Maybe he has a doubt about the electrode or something like this.

Regards 

RAJESH PATNAIK

unread,
Nov 29, 2022, 11:55:20 PM11/29/22
to material...@googlegroups.com
Dear Gents,

This is client spec requirements in most of the companies, as per KOC , we generally do button test
To confirm chemical composition of low alloy and high alloys electrodes per heat.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKL%3DdYw73OyFYLq4yTHUB2cVqbuaDCCunxc73%2BaU0kJZurJd%2Bw%40mail.gmail.com.
--
Thanks & Regards,
RAJESH PATNAIK PITTADA.
Mobile : +919573410309 
              

Faisal Quadri

unread,
Nov 30, 2022, 12:48:21 AM11/30/22
to material...@googlegroups.com
Dear 
See how you will ensure at the receiving stage you received the correct alloy material(Consumables) tell me ????
The weld button is like a test coupon where the PMI probe can easily seat and you can verify the chemistry.

I am working on ARAMCO specs, for us it's mandatory requirement

due to PMI prob inaccessibility on material like consumables and weld , weld button is alternate, in Aramco Spec

check ASME /ASTM for PMI requirements.



Faisal. Q

Sr.Mechanical Inspector,

 

ENERGY & INDUSTRY DIVISION

Dhahran, 34247-2958

Kingdom of Saudi Arabia.

M: +966 537134558

E: faisal...@applusvelosi.com

 


 

 



K Dinesh

unread,
Nov 30, 2022, 2:36:29 AM11/30/22
to material...@googlegroups.com
Hi Ponni,

Check ASME Sec.II Part C SFA 5.9. Annex Clause A5

Thanks & Regards

K.Dinesh 

Metallurgist


P.O. Box 1197, P.C 130, Muscat, Sultanate of Oman

Tel:  +968 24501524, 24505590 (Ext.42), Mob: +968 99880633, Fax: +968 24503814

Email: dinesh@lonestaralpha.com , Web: www.lonestaralpha.com , Location: Click here for Location Map

Locations: Muscat, Sohar, Duqm, Salalah & Liwa

Lonestar now does Pesticide Residues Testing in our new facility at Liwa!

 Consider your environmental responsibility. Think before you print.



Sham Shahabuddin -Welding Inspector, HANBO

unread,
Dec 14, 2022, 11:06:37 PM12/14/22
to material...@googlegroups.com
Dear Mr. Ponnni

If the Filler Metals are provides as per ASME SEC II C then the Test Certificate shall be as per ASME SEC II C requirement of SFA-5.01M/SFA-5.01. No other tests are required as per ASME while receiving the consumables.

Generally for Corrosion Resistant Materials, Clients specify PMI testing of materials at least for a single item in a lot. This is based on the client requirements. 

Thanks & Regards
Sham Shahabuddin