GTAW/SMAW which process is high Heat Input.
 
Thank you
MPK

Raj

unread,
Sep 26, 2011, 12:30:41 AM9/26/11
to Materials & Welding
GTAW is a less heat input process then SMAW.
"Concentrated Arc permits pin point control of heat input to the
workpiece resulting in a narrow heat-affected zone".

Cheers!

Raj

Nimesh Chinoy

unread,
Sep 26, 2011, 1:37:28 AM9/26/11
to material...@googlegroups.com
Dear MKP,

The power at the ARC GAP in 

GTAW = Welding Current * [10 + 0.04x Welding Current]
SMAW = Welding Current * [20 + 0.04x Welding Current] 

So even at the same current level the heat input for SMAW is more than that in GMAW, plus with additional features like Pulsed GTAW, it is easier to reduce the heat input (the same option is not possible in SMAW).

Regards,

Nimesh S Chinoy
SigmaWeld

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Nimesh S Chinoy
Reply all
Reply to author
Forward
0 new messages