Hello Ahmed,

 

Welding procedures for “in Service” welding on pipelines are usually qualified in accordance with API STD 1104, Appendix B. In service welding includes the attachment of repair sleeves, hot tap sleeves, and weld patches. It’s mandated that qualification testing be performed on steels of the same or higher carbon equivalent.

 

Please read through the requirements outlined in Appendix B. The cooling fluid should be flowing water (preferably) due highest quenching effect, resulting the highest hardness values on the pipe wall and the cross section. Simulating 100% of operating conditions is not a requirement. However the welding PQR coupons under water quenching would enforce welding under the worst conditions (especially controlling hardness & hydrogen cracking).

 

B-2.5 outlines the testing requirements, for such Type-B sleeve welds. Required tests are as below.

 

 

Hope this would clarify your doubts.

 

Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Engineering Specialist ,
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 


From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of A Ahmed Ahmed
Sent: Sunday, November 13, 2016 1:00 AM
To: material...@googlegroups.com
Subject: [MW:25673] Inservice PQR Test as per API 1104

 

Dear Expert,

We have one requirement where our Client wants us to carry out Inservice PQR Test as per Annex B on Header Pipe with simulated actual pipeline conditions

 

Is it API 1104 requirement to simulate actual pipeline conditions (Viz Pressure, Temperature, & Flow Rate etc) while carrying Inservice PQR Test

 

Also can somebody guide us on making arrangement which can create / simulate actual pipeline condition by using water as medium.

 

With Best Regards

 

Ahmed

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CA%2BL7tiN-LTZnhkcGUTEXjcAhv6tj_EELnKeGUtiextNtTKm2nA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

image001.gif
Test Coupon Sketch.pdf
Pipeline conditions.pdf
Reply all
Reply to author
Forward
0 new messages