QW-424.2

For welds joining base metals to weld metal buildup or corrosion-resistant weld metal overlay, the buildup or overlay portion of the joint may be substituted

in the test coupon by any P-Number base material that nominally matches the chemical analysis of the buildup or overlay.

With respect to the above clause, Can we approve the following condition.

PQR : P1+ inconel 625 WOL(PWHT) TO P43

Job : P1+Inconel 625 to P1+Inconel 625

Can we use this PQR to weld the Job preparing a WPS accordingly.

Can any one suggest please.

 

Regards

Birupakhya




________________________________________________________________________________________________________________________________
This email may contain confidential and/or privileged information. If you are not the intended recipient (or have received this email in error) please notify the sender immediately and destroy this email. Any unauthorized copying, disclosure or distribution of the information in this email is strictly forbidden.
________________________________________________________________________________________________________________________________

sridhar cn

unread,
Aug 4, 2025, 2:31:31 PMAug 4
to material...@googlegroups.com

Use the PQR if:

The PQR includes Inconel 625 overlay testing (chemical composition, corrosion resistance) on P1.

The job’s weld is primarily between Inconel 625 overlays.

All essential variables (welding process, thickness, etc.) are within the PQR’s qualified range.

You confirm compliance with the project’s code and client requirements.

 

Do not use the PQR if:

The job involves significant base metal welding (P1-to-P1) beyond the overlay, as QW-424.2 may not apply.

The PQR lacks overlay-specific tests or data for Inconel 625.

The project requires a P1-to-P1 PQR.

 

Final Guidance

Draft the WPS: Base it on the PQR, ensuring compliance with QW-424.2 and job requirements.

Consider a New PQR: If the PQR doesn’t meet all conditions or project requirements, qualify a new PQR for 

P1 + Inconel 625 to P1 + Inconel 625 to ensure compliance.


C Sridhar.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/15608E81BA54485586DF9090A788C14E%40temaindia.com.
Reply all
Reply to author
Forward
0 new messages