Dear Group Members,

Base Material : SA 516 Gr 70  
Thickness   : 60 MM
MDMT   : Minus 45 Deg C

Weld consumables Tested for Impact at Minus 46 Deg C
Code : ASME Section 8 Div 1
Joint : Corner Joints
Weld process : GTAW + SMAW + SAW

Designer says : Weld metal exempt as per UCS-67-a-3

Question :

Requirement of Impact test on WPS  ?
Requirement of Production test coupons ?

Raghuram Bathula

unread,
Jun 9, 2015, 2:33:36 AM6/9/15
to Materials-Welding
Given combination is not exempted from Impact testing (Fig UCS-66M)
For PTC your designer need to classify (which category?) whether these are as per Fig UW13.2 or covered by U2(g) as angle joints (with α > 30 ° as per UW3)

k c

unread,
Jun 9, 2015, 4:11:51 AM6/9/15
to material...@googlegroups.com
Yes Mr Raghuram

Joint designed as per UW 13.2 -C

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADxVub%3DrJ8LiKm5iwW4oou5XJT0bOpMVoJdMgk99pxNrha8ZwA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

james gerald

unread,
Jun 9, 2015, 4:32:04 AM6/9/15
to material...@googlegroups.com
Consider the Material is Normalised or Quenched & Tempered, it falls under Curve D. According to Table UCS-66, for 60mm Thk, any temperature less than
-17degC requires Impact Testing of both Base Metal & WeldMetal. Hence for Temperature of -46degC, 60 mm thk requires Impact testing.

For Corner Joints, minimum thckness Applies. Please provide the actual thickne

Production Impact Test is required for Weld & HAZ

1. For each welding procedure used for Category A Joint.
2. Different welding procedure used for Category B Joint other than category A.
3. For SAW welding for each position


Thanks & RegardsJ.Gerald Jayakumar0091-9344954677

--------------------------------------------
On Tue, 6/9/15, k c <kcrtec...@gmail.com> wrote:

Subject: [MW:23062] Clarification on Impact test of WPS and Prduction welds_ASME Sec 8 Div 1
To: material...@googlegroups.com
Date: Tuesday, June 9, 2015, 6:52 AM

Dear Group
Members,
Base Material : SA 516 Gr 70  
Thickness   : 60 MMMDMT   : Minus 45
Deg C
Weld consumables Tested for Impact at Minus 46
Deg CCode : ASME Section 8 Div 1Joint
: Corner JointsWeld process : GTAW + SMAW +
SAW
Designer says : Weld metal exempt as per
UCS-67-a-3
Question :
Requirement of Impact test on WPS
 ?Requirement of Production test coupons
?



--

You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails
from it, send an email to materials-weld...@googlegroups.com.

To post to this group, send email to material...@googlegroups.com.

Visit this group at http://groups.google.com/group/materials-welding.

To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAL9TLdfbnwak067qFAbtfCdfCJ8ZObNLm65iviR3xDpkZ7gCVg%40mail.gmail.com.
Reply all
Reply to author
Forward
0 new messages