Hi
Please use following formula to calculate Preheat temp.
Preheat temperature in Degree celcius = 350 * Square root of (C.E – 0.25 )
Where C.E = CC + CT
CT = CC * 0.005 * T
T = thickness of plate in mm
CC = C + Mn/6 + Ni+Cu/15 + Cr+Mo+V/5
Regards
Prem S Nautiyal
Godrej,Plant 9/19,Mumbai
On Mon, 27 Apr 2009 sandy kumar wrote :
>Can anyone please provide me formula to calculate preheat required for any
>material?
>
>Thanks
>Sandy
>
>>
Hi
This calculation as given below is used but is extremely conservative resulting in much higher preheat temperatures than what is actually required. This impact on costs negatively.
Regards
John du Plessis
Technology Manager
Southern African Institute of Welding
+27 11 2982103 (T)
+27 11 8364132 (F)