PWHT

48 Aufrufe
Direkt zur ersten ungelesenen Nachricht

prateik tolani

ungelesen,
26.02.2020, 09:58:3126.02.20
an material...@googlegroups.com
Dear Experts,

one of our client is asking for Solution annealing for complete vessel
vessel size - 1300 ID x 6500 mm long, thickness 8 mm with lots of nozzles.
whether it is possible.
at higher temperature of 1100 Deg C and rapid cooling in water, vessel will distort completely.


Tolani 

harenath jha

ungelesen,
26.02.2020, 22:24:0926.02.20
an material...@googlegroups.com
Material of construction please

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAGNY-_B7ijqhsdu07O8_05RXO4bHD8%3D%2BGpUx9W68j--H_ZMXQQ%40mail.gmail.com.

james gerald

ungelesen,
26.02.2020, 22:24:1126.02.20
an material...@googlegroups.com
Interesting. What is the material and process Fluid service.

Thanks & Regards

J.Gerald Jayakumar




--

Eyup Tan

ungelesen,
27.02.2020, 00:22:2627.02.20
an material...@googlegroups.com
It looks material is INCONEL 617 or similar. We did the same heat treatments, heating rate 150C/hr holding temp 1100C holding time 1 hr and uncontrolled cooling in air not in water. 

Eyup Tan

iPhone’umdan gönderildi

'james gerald' via Materials & Welding <material...@googlegroups.com> şunları yazdı (27 Şub 2020 06:24):



Kannayeram Gnanapandithan

ungelesen,
27.02.2020, 00:22:2727.02.20
an materials-welding
U have to do like sprinkle type flow on the vessel. Do not immerse or forced water flow on the because it will get collapsed. Be cautious in designing your type of water flow. It is very important. 

Kannayeram Gnanapandithan

ungelesen,
27.02.2020, 09:11:1027.02.20
an materials-welding
Material of construction may be ASS??

--

Kannayeram Gnanapandithan

ungelesen,
27.02.2020, 09:11:1327.02.20
an materials-welding
What is the purpose of solutions annealing for Inconel 617. Generally it is being used for high temperature service

Eyup Tan

ungelesen,
27.02.2020, 10:40:0027.02.20
an material...@googlegroups.com
That is correct The inconel 617 material were used in gas turbine After 33000 hours operation both pieces inner casing and combustion chambers needs to stress relieves. That is why heat treating periodically

Regards 
Eyup Tan 

iPhone’umdan gönderildi

Kannayeram Gnanapandithan <kgpan...@gmail.com> şunları yazdı (27 Şub 2020 17:11):



prateik tolani

ungelesen,
02.03.2020, 02:02:1602.03.20
an material...@googlegroups.com
MOC : SA 240 Gr 316L
Service: WET sour/H2

Pankaj Kolhe

ungelesen,
05.03.2020, 01:39:2305.03.20
an materials-welding
Allen antworten