Radiography requirement of Annular Plate butt welded joint of the Tank / API 653/650

993 views
Skip to first unread message

Vino Varghese

unread,
Apr 14, 2017, 1:33:55 AM4/14/17
to material...@googlegroups.com, Santosh Gaikwad, Raghuram Bathula


Dear Experts,

Tank Material - Group 1
Diameter of Tank - 15 meters

Inspection Recommendation - Replacement of Annular Plate wherever thickness loss observed. Mostly 70% Area will be replaced. Currently the Full Bottom Plate replacement is not feasible. 

Configuration of Weld Joint - Single Butt welded joint with backing strip for the Annular Plate joint.

Query 1: Whether Radiography will be required for the butt welded joint as per API 650, Section 8.1.2.9? 
Query 2: If RT will be required and if it is not possible, whether UT can be taken.

Hope to see the response with respect to Code and request specific answer against both the queries.

Thank you
Regards, Vino




Vino Varghese

unread,
Apr 14, 2017, 1:35:03 AM4/14/17
to material...@googlegroups.com

Prasad Rode

unread,
Apr 16, 2017, 2:29:17 AM4/16/17
to Materials & Welding
Ans1) yes, spot radiography is required with 50% on radial joints.
2) pls check appendix U for the same.

Vino Varghese

unread,
Apr 16, 2017, 9:37:05 PM4/16/17
to material...@googlegroups.com
Dear Prasad

Thanks for the response. However, I understand that Section 8.1.2.9 does not refer to RT requirements for Group 1 materials. In that case RT won't be required for butt welded Annular Plate I believe. 


Thanks and Regards 
Vino 
Qatar 




On 16/04/2017 9:29 AM, "Prasad Rode" <puro...@gmail.com> wrote:
Ans1) yes, spot radiography is required with 50% on radial joints.
2) pls check appendix U for the same.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/7b98fc88-8322-40ea-8ec1-92e8a245b299%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Perumal Govindan

unread,
Apr 17, 2017, 12:28:26 AM4/17/17
to material...@googlegroups.com

Hi

I believe you are repairing the tank.

If so, as per clause 12.2.1.4 of API 653, each annular plate joints shall be radiographed where the shell course rests on the annular plate.

Regards
Govindan Perumal