Transverse Crack on Parent Metal (SS201)

64 views
Skip to first unread message

G Gughan

unread,
Sep 11, 2023, 11:22:28 PM9/11/23
to material...@googlegroups.com

Dear Experts,

 

Please find the attached picture for your deep & clear interpretation. After welding I have found a few transverse cracks along the weld. What could be the reason behind this? Kindly do technical advice or prevention for my understanding.

The material spec is SS201.

Is it a Material defect or a Crack formed due to welding?

Crack induced after a few days of welding not during welding & after immediate welding.

Kindly note that the pipe was formed/developed from the plate by the cold rolling.

 

Your advice & comments will be highly appreciated.

 

Thanks,


Kind Regards,


G.Gughan

IMG_1990.jpg
IMG_1988.jpg

Ahmed Osman

unread,
Sep 12, 2023, 1:29:59 AM9/12/23
to material...@googlegroups.com
is this longitudinal weld ?

This may be stress corrosion crack
* stresses from plate rolling and thermal weld stresses
* corrosion as it is appear in photo ( black spots ) and may be used tools containing halides ( marking colors ) .
* annealing after welding is very effective solution for reducing the tendency of stress cracking 
* pickling did after welding ?  

Best Regards ,
ENG. Ahmed Osman



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB0bcTMTibU4bn1OQy-%3DtoHQ3N2DpTVM4nxJ3NmMfumzqfr_9w%40mail.gmail.com.
Reply all
Reply to author
Forward
0 new messages