Difference between impact testing by ASTME23 and ASTM A370

2,575 views
Skip to first unread message

Vikas Bhandari

unread,
Feb 28, 2011, 7:26:47 AM2/28/11
to material...@googlegroups.com
Dear all, 

I have a procedure in which impact testing should have been done as per  ASTM A370 but it has been done as per ASTM E23

Is there any difference between the standard on how the impact tests are conducted? Would the difference effect the final values?
tha material was UNS 31803 pipe and was tested at minus 50 degree centigrade.

Thanks

jignes...@linde-le.com

unread,
Mar 1, 2011, 2:16:10 AM3/1/11
to material...@googlegroups.com

Dear Mr. Vikas,

A 370 and E 23 both are standard test method for notched bar impact testing of metallic material.

However, there are some basic differences.

A 370 is limited to Charpy V notch impact test specimen. (single Beam)

E 23 covers Charpy (single beam) and Izod ( Cantilever beam) test. Further, Impact testing machine as per A 370 is required to be calibrated as per E 23 ( Direct and/or Indirect methods)

Coming back to your query, just check up is it Charpy test (single beam) or Izod test(cantilever)  as per E 23 ?

Product forms certified as per ASME calls for impact testing as per SA 370. ASME Section IX requires impact testing of material as per SA 370 only.

Also refer your code of construction and applicable customer's specification in order to conclude further.

With Best Regards,

Jignesh R Rana
Manager - Materials Technology, QA/QC & Standards

Linde Engineering India Pvt. Ltd.
'Linde House'
Opp: VUDA Office, VIP Road, Karelibaug,Vadodara - 390018, India.
Tel.: +91 265 3056789, Fax: +91 265 2335213 , Mobile:  +91 90999 86019
jignes...@linde-le.com, www.linde-india.com

This e-mail is confidential. If you are not the intended recipient, please notify us immediately. You should not disclose its contents to any other person nor use it for any purposes.





Vikas Bhandari <vikas.bh...@gmail.com>
Sent by: material...@googlegroups.com

28/02/11 17:56


To
material...@googlegroups.com
cc
Subject
[MW:10058] Difference between impact testing by ASTME23 and ASTM A370


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

ravi

unread,
Mar 1, 2011, 5:07:36 AM3/1/11
to material...@googlegroups.com, jignes...@linde-le.com
Dear Mr Vikas,
Apart from type of Impact test also check for the specimen size.
 
Because A370 provides charpy-V notch test acceptance criteria for sub-size specimens and Table 4.15 of describes the tempearute drop for sub size specimens.
Regards,
Ravi Kumar