PWHT REQUITEMENT AS PER ASME Section VIII Div.1 UCS-56

164 views
Skip to first unread message

Ch Bilal jovinda

unread,
Oct 22, 2025, 9:57:31 PM10/22/25
to material...@googlegroups.com
Dear Team,

  I want to confirm about the PWHT requirement in carbon steel pressure vessel as per ASME section Viii Div.1 UCS-56. Soaking time has been calculated as per vessel wall thickness 29mm but trunion wall thickness is 50mm welded with shell. Can this 50mm thikness be exluded from PWHT soaking time requirement. 
1.Is there any interpretation to confirm that PWHT parameters shall be calculated as per shell wall thickness only not for attachment welded with pressure parts?
2. Below para is applicable for PWHT requirement.




Best regards,
M Bilal

Mohd Siraj

unread,
Oct 23, 2025, 11:08:41 AM10/23/25
to Materials & Welding
by sketch, its joint between 22mm and 50mm ?

so consider thickness 22mm butt weld and beyond above is fillet joint.

Bala Murugan

unread,
Oct 23, 2025, 11:36:01 AM10/23/25
to material...@googlegroups.com
Dear Bilal,
No, you cannot simply ignore the 50 mm trunnion when deciding PWHT. ASME VIII-1 (UCS-56 and related notes/interpretations) makes the pressure-retaining part control the PWHT temperature, but the thickness at the weld/attachment and the weld volume (soak band) are explicitly used to determine heating rate and holding/soaking time. In practice you must check UCS-56 and the ASME interpretations and use the greater thickness condition required by the Code rules for the weld/joint when sizing soak time (and ensure the soak band contains the weld and HAZ)  

Thanks,
Balamurugan

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/ed05ee2b-bc27-4391-82eb-32886ca2700en%40googlegroups.com.

Prem Nautiyal

unread,
Oct 23, 2025, 12:19:19 PM10/23/25
to material...@googlegroups.com
Please proceed with PWHT considering 50mm butt weld size thickness of Trunion ..

Regards

Prem Nautiyal 
Mumbai, India 

Mohmmed Dudhiyawala

unread,
Oct 27, 2025, 12:39:34 AM10/27/25
to Materials & Welding
Dear Bilal,
Refer to Sec VIII Div. 1, UW-40 (f)5f, the governing thickness for PWHT calculation for Non pressure # Pressure Part is the thickness of the weld at the point of attachment. Request calculate Soaking time as per the same.
From attached image, it is appearing as a Groove weld across the thickness. 

Regards,
Mohammed 

venkateswara reddy Desireddy

unread,
Oct 27, 2025, 2:12:36 AM10/27/25
to material...@googlegroups.com
UW-40.6 given how determined PWHT think. Base on that 50mm need to consider for PWHT.




From: material...@googlegroups.com <material...@googlegroups.com> on behalf of Mohmmed Dudhiyawala <mdudh...@gmail.com>
Sent: Monday, October 27, 2025 7:39:27 am
To: Materials & Welding <material...@googlegroups.com>
Subject: Re: [MW:35872] Re: PWHT REQUITEMENT AS PER ASME Section VIII Div.1 UCS-56

Ramesh Barot

unread,
Oct 29, 2025, 12:20:00 AM10/29/25
to material...@googlegroups.com
All are request to clear the same within ASME B31.3 case is as mention below.

1. Trunion thk is 28 mm and mother pipe thk is 23 mm.
2. Type of joint fillet joint

PWHT required or not?

Muhammed Ibrahim PK

unread,
Nov 9, 2025, 2:26:09 AM11/9/25
to material...@googlegroups.com
Hi,

It was in my project. We concluded it required PWHT soaking time for 50 mm (2 hrs) as the part directly welding with the shell is 50 mm. Here 50 mm will be governing thickness.

Even we make direct fillet weld throat thickness more than 38 mm will call for PWHT.

Thanks & Regards
Muhammed Ibrahim PK


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Reply all
Reply to author
Forward
0 new messages