Corrosion in CRA pipes

139 views
Skip to first unread message

berry gamaliel

unread,
Mar 12, 2016, 10:57:32 PM3/12/16
to material...@googlegroups.com
Dear Experts 

In our project we are using CRA pipes, API 5L Grade B, thk- 35 mm. cladded with UNS00825  thk-5mm. 

Due to improper preservation of spools grinding and machining wastes deposited or setteled inside the spools and oxidation and corrosion started in a minor way. 

Please suggest whether chemical cleaning is required to to remove the minor corrosion or as it is a corrosion resistance alloy pipes will it withstand the corrosion. 

Another clarification too as it is a Corrosion resistance alloy why it cannot resist or prevent corrosion from grinding and machine wasted and during the service condition highly corrosive fluids will pass though it so how it will withstand that. 

Please clarify experts. 


--
Regards


Berry Gamaliel





--
Regards


Berry Gamaliel


Alan Denney

unread,
Mar 13, 2016, 5:40:35 AM3/13/16
to material...@googlegroups.com

I understand that the designer has selected alloy 825 (as internal cladding) as adequate for the in-process service and you are asking why you have to remove swarf, from within the pipe. Since the swarf is from cutting a clad pipe it will be largely carbon steel. The reason is that the alloy 825 relies on a layer of passive surface scale to make it corrosion resistant. The swarf will set up a galvanic corrosion cell, assisted by the crevices formed under the corrosion product, the protective layer will be breached by the corrosion the surface will be pitted and corrosion can proceed in the pit regardless of what is done to the surface. I suggest you search for the terms, galvanic corrosion, pitting corrosion and crevice corrosion to understand the risks being created. The requirement that you prevent the ingress of swarf is correct.

 

Alan Denney

AKD Materials Consulting Ltd

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKN5ewYsLRKgL0NyDp4_UYcQTBkiHk5ZF1-S--%2BbRmoup8Xukg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


This email has been scanned by BullGuard antivirus protection.
For more info visit www.bullguard.com

dili...@gmail.com

unread,
Mar 13, 2016, 8:58:56 AM3/13/16
to berry gamaliel
If the cladding has been contaminated by iron then you have to perform smooth grinding and pickling

Sent from my BlackBerry 10 smartphone.
From: berry gamaliel
Sent: Κυριακή, 13 Μαρτίου 2016 - 05:57
Subject: [MW:24509] Corrosion in CRA pipes

Ahmed Eissa

unread,
Mar 13, 2016, 11:35:53 PM3/13/16
to material...@googlegroups.com
Ni based alloy 825 is used to mitigate certain damage mechanisms, however fabrication of these alloy shall be performed with due care (similar to duplex and super duplex) 
Please avail service data,  handled stream,  I suggest hydrocarbon with produced water or water injection service 

A.E
Material and corrosion engineer 

Sent from Yahoo Mail on Android


From:"berry gamaliel" <mechberr...@gmail.com>
Date:Sun, 13 Mar, 2016 at 5:57 am

Subject:[MW:24509] Corrosion in CRA pipes

Alan Denney

unread,
Mar 13, 2016, 11:36:06 PM3/13/16
to material...@googlegroups.com

 

Alan Denney

AKD Materials Consulting Ltd

 

From: Ahmed Husain [mailto:ahm...@yahoo.com]
Sent: 13 March 2016 15:52
To: material...@googlegroups.com; Alan Denney <al...@denney1.freeserve.co.uk>; material...@googlegroups.com
Subject: Re: [MW:24517] RE: 24509] Corrosion in CRA pipes

 

As per my understanding, in galvanic corrosion, material listed lower in galvanic table is the one which should deteriorate. In this case, cs is the lower grade and should deteriorate, not the alloy 825. 

In all carbon steel piping, gasket winding and inner rings is normally SS, but there is no issue of galvanic corrosion.

I think, this issue of contamination should require more discussion.

 

Regards,

Ahmed

On Sun, 13 Mar, 2016 at 12:29 pm, Alan Denney

Ahmed Husain

unread,
Mar 13, 2016, 11:36:17 PM3/13/16
to material...@googlegroups.com, Alan Denney
As per my understanding, in galvanic corrosion, material listed lower in galvanic table is the one which should deteriorate. In this case, cs is the lower grade and should deteriorate, not the alloy 825. 
In all carbon steel piping, gasket winding and inner rings is normally SS, but there is no issue of galvanic corrosion.
I think, this issue of contamination should require more discussion.

Regards,
Ahmed
On Sun, 13 Mar, 2016 at 12:29 pm, Alan Denney
Reply all
Reply to author
Forward
0 new messages