Dear Mishra
Pl refers your contract documents for acceptance. However we can control the distortion by using following method,
— Minimum welding current as per WPS.
— Intermittent welding
— Do not over weld
— Design welds location near the neutral axis.
— Balance the weld around the neutral axis
— Sequence welding
— Pre bending OR Pre cambering
— Back to back clamping
— Double operator welding technique
— Keep the angle of weld joint to the barest minimum.
— Minimize No of passes using larger size of electrodes
TR
Meeran
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-weld...@googlegroups.com.
To post to this group, send email to
material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/193acce9-526e-435b-b32d-734022c05144%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
|
This Message and its contents is intended solely for the addressee and is proprietary. Information in this mail is for L&T Business Usage only. Any Use to other than the addressee is misuse and infringement to Proprietorship of L&T Construction. If you are
not the addressee please return the mail to the sender. L&T Construction. |