Transverse crack observed after fillet welding

95 views
Skip to first unread message

kishore barbudhe

unread,
May 15, 2022, 11:13:34 PM5/15/22
to welding
Dear expert,

We observed transverse cracks after completion of fillet welding.
We are using EA2 filler wire in submerge arc welding and parent materials is E 450.
Please give us advice to resolve this issue.

Thanks & Regards

Kishore B 

Vishwas Keskar

unread,
May 16, 2022, 12:01:09 AM5/16/22
to material...@googlegroups.com
Which flux/ wire brand  is used?
What is Fillet size?




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1190457571.2472505.1652533602689%40mail.yahoo.com.

Prakash Hegde

unread,
May 16, 2022, 1:19:24 AM5/16/22
to material...@googlegroups.com
Hi
There is a tendency of Cracks in Fillet weld 
if
Set up is not proper I. e  uneven at matching /mating  surface causing distortion
There should be strong tack weld on both ends and on opposite sides
Improper st up causes heavy stresses on weld causes cracks
 Regards
--

kishore barbudhe

unread,
May 16, 2022, 2:34:04 AM5/16/22
to material...@googlegroups.com
Hi, 
during fit up 100 mm tackweld done on both side joints. i observed that after 1st pass i was check LPT after 24 hrs & found there is no crack. but, after 3rd pass of welding observed transver cracks overall 12 meter length

Regards
Kishore B 

Ahmed Osman

unread,
May 16, 2022, 3:50:59 AM5/16/22
to material...@googlegroups.com
Dears ,
Mo. in EA2 wire have a tendency for hardness increasing after reheating especially with active flux ,
u can try to use neutral flux or use Mn Si wire

Best Regards ,
ENG. Ahmed Osman


james gerald

unread,
May 16, 2022, 3:59:31 AM5/16/22
to 'kishore barbudhe' via Materials & Welding
It seems to be like Hydrogen cracking.

1. Check whether your SAW Flux Baked properly in recommendation with Manufacturer.
2. Clean the weld surface free of oil, Grease, Paint etc..
3. Check the ratio of mixing old flux recovered after welding with new Flux.

Thanks & Regards

J.Gerald Jayakumar





Prakash Hegde

unread,
May 16, 2022, 4:54:34 AM5/16/22
to material...@googlegroups.com
Thkness of tack weldshould be thicker 
And no gap in fit up
Preheat is prefered
On Mon, 16 May 2022 at 12:03, 'kishore barbudhe' via Materials & Welding

james gerald

unread,
May 16, 2022, 5:07:25 AM5/16/22
to 'james gerald' via Materials & Welding
Hydrogen cracking is because of below.

1. Presence of Hydrogen. (By proper Baking of Flux for SAW and a clean environment can be reduced).
2. Susceptible Microstructure like Martensite (which can be prevented by Preheating and Heat Input)
3. Stresses (May be Internal or External, by proper alignment using Tacks and reducing the cooling rate it can be avoided).


Thanks & Regards

J.Gerald Jayakumar


pgos...@rogers.com

unread,
May 16, 2022, 8:09:06 AM5/16/22
to material...@googlegroups.com

Hi Kishore,

 

What’s the width of the fillet weld at the 3rd pass?

Is you welder trying to deposit a single pass fillet weld for the capping pass or following a multi-pass weld to finish the capping run.

What’s the voltage involved?

If the width is typically > 4 x Core Wire Diameter , with higher voltage say > 35V , centerline cracking in SAW welds may occur.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232




AVG logo

This email has been checked for viruses by AVG antivirus software.
www.avg.com


Reply all
Reply to author
Forward
0 new messages