We welded a 15E Pipe material (16 inch - 87mm thickness).
Our procedure will be preheated with 205 deg centigrade then welding and will be
( hydrogen ) bakeout and perform PAUT, If accepted in PAUT, immediately followed
by PWHT and will perform MT.
Process is B31.1

The joint has been accepted by PAUT, my query is, how long should be acceptable if there is a delay in performing PWHT?
Right now it is almost 1 week that the welded joint is not yet PWHT.

Need your advice.

pgoswami

unread,
Feb 25, 2016, 11:59:08 PM2/25/16
to material...@googlegroups.com

Hi Mac,

 

One week without PWHT on 3.5” think Grade -91 Steel is too long. In spite of hydrogen bake out one may get cracking. Did any one check the hardness of weld and HAZ by any means (just for curiosity??).

 

Also prior to the DHT the welds should be cooled to Mf   temperature which is generally  the ambient temperature. In absence of it full martens tic transformation won’t happen causing poor creep strength in these steels. DHT may be adopted before the PWHT, however not advised to delay PWHT so long.

 

It’s worth looking at.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 

 


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2273403b-7345-464c-8e91-93d53134f4f8%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

image001.gif

Lakshman

unread,
Feb 26, 2016, 12:41:27 AM2/26/16
to material...@googlegroups.com

Hi Mr. Pradip Goswami,

 

Thanks a lot for the info,

Shall we need to reconfirm the soundness of the weld and HAZ area by any means of NDT prior to PWHT once again? As it was delayed for more than a week, any specific requirements are their?

I’m not connected to this subject, but for my information  I am requesting you….

 

Thanks & Regards,

Lakshman Kumar B,

+91 9440031459.

image001.gif

c.no...@vipco-thai.com

unread,
Feb 26, 2016, 12:49:17 AM2/26/16
to material...@googlegroups.com

Once our shop got a relax from client to keep it as long as one week if the storage was done with assurance that relative humidity would be low and not create risk of cracking due to water.

What we did during that time was using heater in storage shade and monitoring humidity.

Anyhow,  no body is comfortable to see 15E welded joint stayed without PWHT too long.  PT/MT and volumetric inspection after PWHT is highly recommended.

Regards,

C.Nopadon

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of pgoswami


Sent: Friday, February 26, 2016 11:59 AM
To: material...@googlegroups.com

image001.gif

John Henning

unread,
Feb 26, 2016, 9:34:16 AM2/26/16
to material...@googlegroups.com

what were the storage conditions.  If pipe is being kept dry there should be no problem.  The concern with delay is the possibility of SCC if the the as welded material gets wet.  Wet in this case means any water including dew formation.  Been a lot of discussion on this issue in the past.  In 30 years of experience I have not seen any evidence of as welded cracking  as long as there was controlled storage.




From: material...@googlegroups.com <material...@googlegroups.com> on behalf of pgoswami <pgos...@quickclic.net>
Sent: Thursday, February 25, 2016 10:58 PM
To: material...@googlegroups.com
Subject: [MW:24374] RE: 24373] Time between Hydrogen Bake Out and PWHT
 

Michael J Crichton

unread,
Feb 27, 2016, 12:01:25 AM2/27/16
to material...@googlegroups.com

B31.1 requires NDE to occur after PWHT for P15E materials.  Section 136.4 “…NDE for P-Nos. 3, 4, 5A, 5B, and 15E material welds shall be performed after postweld heat treatment unless directed otherwise by engineering design.”

 

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of John Henning
Sent: Friday, February 26, 2016 9:34 AM
To: material...@googlegroups.com
Subject: Re: [MW:24377] RE: 24373] Time between Hydrogen Bake Out and PWHT

 

This is an EXTERNAL email. STOP. THINK before you CLICK links or OPEN attachments.


Ramdoss Ravindiren

unread,
Feb 27, 2016, 12:01:37 AM2/27/16
to material...@googlegroups.com
Dear all,

As a good engeering practice,  PWHT shall be done asap after completion of welding.

In unavoidable circumstances PWHT can be done even after 14days provided

1. Weld shall be free from moisture.
2. Weld shall not be subjected to any load.

Regards,
Ramdoss
Doosan

From: John Henning
Sent: ‎26-‎02-‎2016 08:04 PM

To: material...@googlegroups.com
Subject: Re: [MW:24377] RE: 24373] Time between Hydrogen Bake Out and PWHT

Mac Palola

unread,
Feb 27, 2016, 12:02:17 AM2/27/16
to Materials & Welding
Sir,

The plan for HARDNESS TEST is after PWHT. If we do hardness test before PWHT,
what can we distinguish then?

Doc1.docx
Auto Generated Inline Image 1

Kannayeram Gnanapandithan

unread,
Feb 27, 2016, 12:02:57 AM2/27/16
to material...@googlegroups.com

After hydrogen bake out, it should not be more than 72 hrs without PWHT. Environment should be dry, no physical movement. It always better to do pwht as early as possible, such a heavy thick not advisable. Check all NDT before taking for PWHT

pgoswami

unread,
Feb 27, 2016, 12:19:48 AM2/27/16
to material...@googlegroups.com, c.no...@vipco-thai.com, lakshma...@gmail.com

Hi Mr Lakhsman and Mr Nopadon,

 

Thanks for your query and thanks to Mr Nopadon for sharing his experience.

 

Usually 3 factors contribute to SCC, which had been observed for Grade -91 steel  in specific instances (please see below):-

 

  • Stress .High residual  tensile stress  is prevalent in untempered or Non PWHT-ed grade 91 welds. This is a significant factor  to generate cracking.

 

  • Specific environment: Humid environment , close to coastal areas ( where the salinity is always high) could be a contributing factor for generating SCC. Also SCC   significantly accelerates when the ambient temperature is always  high 20 Deg C or more for  grade 91 steel.

 

  • Also CSEF steels e.g. grade-91 steel does not have enough resistance to SCC.

 

The as welded hardness in this steel is easily above 300-350 HV or more, hence leaving thus steel untempered , in any of the above environments would aggravate the  probability  of cracking .It’s the precise reason for controlling environments in case the PWHT is delayed.

 

People often talk about DHT:- DHT is good to mitigate the probability of Hydrogen cracking. This would work better even when the welding consumables are strictly H4 category or less (see attached). However performing DHT alone and delaying the PWHT does not solve all “cracking propensities” for this grade of steels.

 

These are my thoughts, which may be conservative. But cracks in Grade-91 steel could be a nightmare and needs to be avoided at all costs.

 

Please see highlighted text in the attached publication from TWI. Though written for Grade-92 steel, all rules are the same forGrade-91 also.

 

Thanks

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 

 

 

Stress Corrosion Cracking Triangle

 

 

 

 

 

 

 

 

 

 

 

___________________________________________________________________________________________________________________________________________________________________________________________________________________________________________________

 Hi Mr. Pradip Goswami,

 

Thanks a lot for the info,

Shall we need to reconfirm the soundness of the weld and HAZ area by any means of NDT prior to PWHT once again? As it was delayed for more than a week, any specific requirements are their?

I’m not connected to this subject, but for my information  I am requesting you….

 

Thanks & Regards,

Lakshman Kumar B,

+91 9440031459.

 

 

To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/005e01d17059%241ad91690%24508b43b0%24%40vipco-thai.com.
image001.gif
image002.gif
Consonni & Mathers - Welding & Cutting 01 2012.pdf
SL9crp91-ENG.pdf
Reply all
Reply to author
Forward
0 new messages