Auto Tig for SS 310 with Ar+H2 gas

62 views
Skip to first unread message

Hrushikesh Sangamnerkar

unread,
Oct 20, 2022, 11:12:52 PM10/20/22
to Materials & Welding
Dear experts,

Query is can we weld Auto Tig (with Filler) for gas combination of Ar+Hydrogen? Pl provide technical literature to support the question,if available at your end.

Currently facing an issue of LOP with Argon gas only..

Regards,

Vishwas Keskar Welding Manager WELDING

unread,
Oct 20, 2022, 11:53:10 PM10/20/22
to Materials & Welding
What is  joint configuration and thickness?

james gerald

unread,
Oct 21, 2022, 5:21:29 AM10/21/22
to material...@googlegroups.com
Use the below chart.

Inline image


Thanks & Regards

J.Gerald Jayakumar




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMpWL2piyXRMx4A4tXavwmxnn-6dO4PkfAEZzw%2B4Cwd15h4TmA%40mail.gmail.com.

Hrushikesh Sangamnerkar

unread,
Oct 24, 2022, 11:51:21 PM10/24/22
to Materials & Welding
Thanks for the input.

Can you share the technical backup with the specific grade of SS..

Hrushikesh Sangamnerkar

unread,
Oct 24, 2022, 11:51:28 PM10/24/22
to Materials & Welding
Single V.. 60 deg included angle.. 0mm root face with 1-1.5mm root gap

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

Kannayeram Gnanapandithan

unread,
Oct 25, 2022, 11:29:13 PM10/25/22
to materials-welding

Nimesh Chinoy

unread,
Oct 25, 2022, 11:56:05 PM10/25/22
to material...@googlegroups.com
Hrishikesh we can use Ar 98% and 2%H2 with Filler wire. We use it for SigmaWeld Accelerated Tig, Square Butt Single Pass for SS310, with Filler.

Please connect will be able to help with some parameters...

We have used similar combination for capping passes as well. Tungsten angle will also play an important role

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

hussain awan

unread,
Oct 27, 2022, 1:30:31 AM10/27/22
to material...@googlegroups.com
Dear All,

Please suggest electrode for welding API 5CT pipe subject captioned Grades 
If any wps is available please provide 

Thanks & Regards
Hussain

Kannayeram Gnanapandithan

unread,
Oct 29, 2022, 1:39:37 AM10/29/22
to materials-welding
adding 2%H2 may give heat input more and clean weld but it may lead to undercutting, it is better go with Argon +Helium mixture. 