Why is preheating important for welding Alloy Steel?

977 views
Skip to first unread message

Suresh Babu

unread,
Jan 7, 2011, 2:50:08 AM1/7/11
to Materials & Welding
Dear Team..i would like to get a correct answer for the following
question.

Why is preheating important for welding Alloy Steel?

Thanks in advance
SURESH.

gohil tushar mansukhlal

unread,
Jan 7, 2011, 3:02:59 AM1/7/11
to material...@googlegroups.com
Dear friend preheating is required to minimise the temperature gradient (difference ) which result in slow cooling of weld bead and HAZ. Rapid cooling of weld and HAZ will result in cracking of weld or HAZ.

Tushar Gohil

On Fri, 07 Jan 2011 13:27:13 +0530 wrote
--

To post to this group, send email to material...@googlegroups.com

To unsubscribe from this group, send email to materials-weld...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Arunachalam A

unread,
Jan 7, 2011, 3:00:41 AM1/7/11
to material...@googlegroups.com

The purpose of preheat:-
Reduce the risk of hydrogen cracking
Reduce the hardness of the weld heat affected zone
Reduce shrinkage stresses during cooling and improve the distribution of residual stresses.

If preheat is locally applied it must extend to at least 75mm from the weld location and be preferably measured on the opposite face to the one being welded.

http://www.gowelding.com/weld/preheat/preheatcalc.htm


Background To Preheating

When hydrogen diffusing from a solidified weld meets a hard microstructure under a tensile stress a crack is likely!

Hydrogen cracking normally occurs in the heat affected zone where hard microstructure is to be found, occasionally it can occur in weld metal.


Hydrogen
This is a very searching gas that can be liberated by oil, grease, rust etc. and water under the right conditions.

The greatest risk comes from hydrogen generated within the arc from damp or contaminated welding consumables, mainly fluxes or electrode coatings.

Contamination on the parent metal can also be a risk unless the heat from the welding arc can drive it away. Moisture from condensation on the parent metal will normally be driven off by the heat from the arc before it can get into the weld pool.

Hydrogen in the atmosphere is unlikely to penetrate the arc envelope unless welding is carried out in very damp and humid conditions.

A hydrogen crack can take anything from a few hours to 24 hours to occur. After 24 hours cracking is still possible but less likely, although there have been some reported cases of cracking at 72 hours. It is therefore good practice to allow at least 48 hours before carrying out any NDE.

Hydrogen will eventually disperse from the parent metal, within a few days at room temperature or a few hours if held at around 200°C.

Hydrogen cracking is only possible at room temperature, this is why it is also referred to as cold cracking


Parent Metal
A hydrogen crack requires a hard microstructure which is created by a hardenable material subject to fast cooling from 800°C to 500°C. Cooling can be slowed down by:-
applying preheat,
maintaining a high interpass temperature,
increasing welding power and reducing travel speed.

The heat sink caused by the parent metal thickness and the number of available paths the heat can take to escape, also influence cooling rate. (However once the heat sink reaches a certain size further increases have a negligible effect on cooling rate.). This is why when determining preheat the term combined thickness is used, for a butt weld it is twice the thickness of the parent material and for a T fillet weld three times the thickness.

The hardening of a carbon manganese steel/low alloy steel is influenced primarily by carbon content and to a lesser extent other constituents such as manganese, chrome, silicone etc.

The Carbon Equivalent is a formula used to express the harden-ability of a particular alloy steel in terms of an equivalent plain carbon steel. Several such formula exist, the one favoured for low alloy steel is the IIW formula:

CEIIW = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Current steel specification do not restrict or limit the Carbon Equivalent and as most steel specs permit a wide range of composition it is possible that one batch of steel may require pre-heat and another may not.

Very low sulphur ( < 0.015%) will increase hardening and special precautions are required when determining the minimum preheat level. Additions of niobium also require special consideration.

For welds subject to high restraint more preheat is advisable (suggest, Increase CE by 0.3 or go down one hydrogen scale).



References.

EN1011 Part 2 (English version available from British Standards)
This standard is highly recommended as it gives details on this preheat method and also includes methods covering fine grain and creep resisting steels. It also includes practical guidance on the avoidance of other cracking mechanisms. Much of the data contained in this standard comes from TWI research tempered by practical experience from industry. (It replaces BS5135)

Welding Steels Without Hydrogen Cracking.


This book is based on the original research work carried out by TWI. It covers the avoidance of hydrogen cracking and preheat in great detail. The preheat graphs tend to require a higher preheat than the equivalent ones in EN1011.

The Welding of Structural Steels Without Preheat The Welding Journal April 2000
A very informative article covering recent TWI research into welding low hardenability steels without preheat. The article won the Lincoln arc welding foundation gold award.

Preheat calculator Lincoln arc welding foundation
A simple to use and inexpensive calculator. It is based on practical experience and tends to be very conservative when compared with the TWI method.


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
அருணாசலம்
கலைவாணி
சுதர்ஷனா
வருண்


keyconcepts1.pdf

Manish Yadav

unread,
Jan 7, 2011, 5:02:21 AM1/7/11
to material...@googlegroups.com
I just wanted to know "PRE HEAT IS REQUIRED IN API 5L PSL-1 AND API 5L PSL-2
MANISH YADAV
08890122779,7877056928

Suresh Babu

unread,
Jan 7, 2011, 5:19:53 AM1/7/11
to Materials & Welding
Dear All,
Thanks for the inputs!.
But still my question is not resolved.
I would like to get a simple answer especially for Alloy
Steel(eg.P11,P22 etc..) why pre heat is required.
As for now i could say ---The heat input provided by welding alloy
steel is not sufficient for keeping the structure as hot as
needed,then external heating means must be implimented to assure the
interpass temperature required.

Regards,
SURESH
> On Fri, Jan 7, 2011 at 11:50 AM, Suresh Babu <suresh75.b...@gmail.com>wrote:
>
>
>
>
>
> > Dear Team..i would like to get a correct answer for the following
> > question.
>
> > Why is preheating important for welding Alloy Steel?
>
> > Thanks in advance
> > SURESH.
>
> > --
> > To post to this group, send email to material...@googlegroups.com
> > To unsubscribe from this group, send email to
> > materials-weld...@googlegroups.com<materials-welding%2Bunsubscr­i...@googlegroups.com>
> > For more options, visit this group's bolg at
> >http://materials-welding.blogspot.com/
> > The views expressed/exchnaged in this group are members personel views and
> > meant for educational purposes only, Users must take their own decisions
> > w.r.t. applicable code/standard/contract documents.
>
> --
> அருணாசலம்
> கலைவாணி
> சுதர்ஷனா
> வருண்
>
>  keyconcepts1.pdf
> 203KViewDownload- Hide quoted text -
>
> - Show quoted text -

vikas kumar

unread,
Jan 7, 2011, 7:07:19 AM1/7/11
to material...@googlegroups.com
PREHEATING IS REQUIRED FOR HIGH ALLOY STEEL LIKE AS P91 MATERIAL , BECAUSE P91 MATERIAL IS CORE GRAIN MATERIAL, WHICH IS MOST HARD MATERIAL, AND THE GRAIN SIZE IS VERY HARD, SO BROKEN OR MELT THIS GRAIN SIZE WE PREHEAT THE MATERIAL AT 250 YO 350C, DEPENDING UPON THICKNESS, OTHERWISE WE DO NOT APPLY PREHEAT ON MATERIALON HIGH ALLOY WELDING CRACK DEFENTLY FOUND.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
Reply all
Reply to author
Forward
0 new messages