Base metal qualification range of unlisted material as per AWS D1.1

1,281 views
Skip to first unread message

shaik amjad

unread,
Oct 31, 2016, 7:08:49 AM10/31/16
to Materials & Welding
If a wps is qualified in base metal S355J2 will it be qulified for S355JR Code AWS. I have WPS qualified with base metal S355J2  but now due to stock availability only S 355JR is available can i use same WPS for this one also . as only the grade is changing  

anthony chundal

unread,
Oct 31, 2016, 7:46:21 AM10/31/16
to material...@googlegroups.com
Dear Shaik,

Please note that S355J2 or JR Materials are unassigned materials without P nos, so you have to qualify with the actual base material in this case.
However you can approach the clients by saying that the yield strength is same and the consumables used also will be same, in that case may be they will accept.

On Mon, Oct 31, 2016 at 2:50 PM, shaik amjad <amjadsh...@gmail.com> wrote:
If a wps is qualified in base metal S355J2 will it be qulified for S355JR Code AWS. I have WPS qualified with base metal S355J2  but now due to stock availability only S 355JR is available can i use same WPS for this one also . as only the grade is changing  

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/288c4978-e27c-4ec3-abac-5ae1f4cb7f53%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

shaik amjad

unread,
Nov 1, 2016, 5:53:57 AM11/1/16
to Materials & Welding
Thanks a lot for the response sir, That was the exact doubt i was having , as  S355 is un listed in AWSD1.1  ,  also The only diffrence between S355J2 and S355JR is the impact test requirement . other properties are same .  

Rajagopal Kannan

unread,
Nov 1, 2016, 6:05:13 AM11/1/16
to material...@googlegroups.com
Hi Amjad,

Sorry. This is the MAIN Issue when AWS D1.1 is used for qualification. I wonder why this code is of such a narrow scope with regards to materials.

Yes, 
a. you need to requalify for J2 Material.
b. If client accepts, Please try performing Impact test of the material per J2 requirements, if successful, it may be recertified to J2 for the particular product. also ensure the chemical properties match J2 Requirements.
c. Ask for concession to use the same WPS from the client.

The main reason I prefer to go per EN ISO 15614 in lieu of AWS D1.1 is this narrow range of materials. EN limits the range based on Material Yield strength not by the designation.

Thanks and Best Regards,
K.Rajagopal


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.