P9B materials welding qualification limit with impact & without PWHT

290 views
Skip to first unread message

kamal nathan

unread,
Feb 7, 2012, 4:32:21 AM2/7/12
to materials-welding
Team members,

Could one give the interpretation clarity of the below :

1.Refer to ASME SEC.VIII .DIV.1 UCS-56 table for P9B materials under
note 3 (a) which states that qualification has to be done in equal or
greater thickness than the production weld thickness(Our customer
specs.(UDHE) also specifies that all welding procedures shall be
qualified on plates not thinner than the part to be welded.)

&

2.Refer to ASME SEC. IX QW-403.6 which states that minimum thickness
qualified is the thicknes of the test coupen or 16 mm whichever is
less .


While comparing the above 2 mentioned statement: Whether we need to
do the welding procedure qualification for each thickness with impact
& without PWHT?


Thanks,
kamal

vijayan

unread,
Feb 8, 2012, 1:59:02 AM2/8/12
to material...@googlegroups.com

Hi

 

 

The note is clear. For material over 16mm thk shall be PWHT with any qualified WPS. But, If the material thickness under question is <16mm, then the PWHT is not mandatory subject to that, the PQR should have been qualified on same or greater thickness than the production thickness.

 

Limitations on essential/supplementary variables per ASME Sec IX shall also to be complied.

 

// While comparing the above 2 mentioned statement:  Whether we need to do the welding procedure qualification for each thickness with impact & without PWHT?//

 

Yes. Instead you can go for PWHT which is economical.

 

 

BR

M.Vijayan

--

To post to this group, send email to material...@googlegroups.com

To unsubscribe from this group, send email to materials-weld...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



This communication and any files transmitted with it are confidential and may also be privileged. It is for the exclusive use of the intended recipient(s). If you are not the intended recipient or the person responsible for delivering it to the intended recipient(s), please note that any form of distribution, copying or use of this communication or information contained in it is strictly prohibited and may be unlawful. If you have received this communication in error please return it to the sender, and delete the material from any computer. We reserve the right to monitor email communications through normal internal and external networks. We believe but not warrant that the email and the attachments are virus free. The statement and opinions expressed in this communication are those of the writer and do not necessarily represent those of Madina Group, whose registered office address is