We have done PQR with PWHT for the Material APL 5L Grade X60, and the coupon Size is 40 Inch & the Thickness is 38 mm with the Construction code application of API 1104 (Cross Country Pipe Line)

Based on the results we prepared WPS Also, But, As per API 1104 for 38.00 mm THK PWHT is not required 

Now The Aramco PID instructed to follow the WPS to do all the Joints PWHT

What is the remdy for this & hat should we do 

Kindly drop your advise 


Thanks & Warm Regards,

Amul Raj T

QA/QC Welding 

Samsung Engg, KSA  



 




Anup N K E

unread,
Mar 5, 2015, 11:02:04 AM3/5/15
to material...@googlegroups.com

Also you can mention in your WPS that the WPS having PWHT is only applicable for thickness above 38mm to the maximum thickness qualified . Please refer SAES W - 012 and SAIC - W- 2042.

Regards,

Anup

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2f252b05-3866-481c-9fcf-2357a5f0c95e%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Anup N K E

unread,
Mar 5, 2015, 11:02:11 AM3/5/15
to material...@googlegroups.com

Dear Amul,

What is the design code.? If it is ANSI B 31.4 or B 31.8  then PWHT is required above 38 mm.
Design code will specify PWHT requirements which is to be incorporated  while making the WPS using section IX or API 1104.

Regards,

Anup

On 5 Mar 2015 13:36, "Amul Raj" <win....@gmail.com> wrote:

S.Mohammed

unread,
Mar 5, 2015, 11:02:52 AM3/5/15
to material...@googlegroups.com

AMUL,

ARAMCO IS RIGHT.

Refer design code for PWHT requirement.

B31.4 OR 31.8.


B31.8 require 32mm PWHT.

you.will have to.do.it pwht for all the joints.

regards,

Faisal Shahzad Meer

unread,
Mar 5, 2015, 11:02:55 AM3/5/15
to material...@googlegroups.com
For PWHT YOU HAVE TO CONSULT B31.4 OR B31.8 WHICH EVER IS APPLICABLE AS PER SAES-W-012 (SAUDI ARAMCO ENGINEERING STANDARD.

Regards

Faisal Shahzad Meer
Project Quality Supervisor-Welding
J-505, Saudi Aramco Wasit Downstream Pipelines Project

[cid:image0...@01CCFE94.22F135F0][cid:image0...@01CC027E.87D3EED0]
TEL :+966 3 6795805-7 Ext. 124|www.gccksa.com<http://www.gccksa.com/>
E-mail fm...@gccksa.com<mailto:msha...@gccksa.com>
[Description: MCj03968400000[1]]+966 - 553919249
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com<mailto:materials-weld...@googlegroups.com>.
To post to this group, send email to material...@googlegroups.com<mailto:material...@googlegroups.com>.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2f252b05-3866-481c-9fcf-2357a5f0c95e%40googlegroups.com<https://groups.google.com/d/msgid/materials-welding/2f252b05-3866-481c-9fcf-2357a5f0c95e%40googlegroups.com?utm_medium=email&utm_source=footer>.
image001.jpg
image002.jpg
image003.png

mv_srinivasan

unread,
Mar 6, 2015, 12:59:07 AM3/6/15
to material...@googlegroups.com
Sir,
which design code is used whether ASME 31.4  or ASME 31.8.


Sent from Samsung Mobile


-------- Original message --------
From: Amul Raj
Date:05/03/2015 11:58 (GMT+03:00)
To: material...@googlegroups.com
Subject: [MW:22939] Requirements Of PWHT for the Cross Country Pipe Lines - Reg

Dear Experts,

We have done PQR with PWHT for the Material APL 5L Grade X60, and the coupon Size is 40 Inch & the Thickness is 38 mm with the Construction code application of API 1104 (Cross Country Pipe Line)

Based on the results we prepared WPS Also, But, As per API 1104 for 38.00 mm THK PWHT is not required 

Now The Aramco PID instructed to follow the WPS to do all the Joints PWHT

What is the remdy for this & hat should we do 

Kindly drop your advise 


Thanks & Warm Regards,

Amul Raj T

QA/QC Welding 

Samsung Engg, KSA  



 




--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

Anup N K E

unread,
Mar 6, 2015, 6:40:39 AM3/6/15
to material...@googlegroups.com

Refer scope of work,  Isometric drawing and P & ID to find the applicable code.
Section 434.8.9 specifies about PWHT is ANSI B 31.4

Regards,
Anup

Karthik

unread,
Mar 11, 2015, 5:28:12 AM3/11/15
to material...@googlegroups.com
Hi,
Since your WPS qu
 
Thanks & Regards,alified with PWHT, you can't use this for without PWHT jobs.
Since your construction code doesn't reqire PWHT you have 2 option.
01. Do new WPS/PQR without PWHT
02. If you don't want to prepare new, then follow as per your existing WPS (as your client said)

(Karthik)




prasanta kumar Sethi

unread,
Mar 16, 2015, 2:41:41 AM3/16/15
to material...@googlegroups.com
Hi as per yr qualified WPS you have to do the PWHT because this is as per code says as well as  ARAMCO .
 
So sorry there is no other option for u. 

Dani Darwis

unread,
Mar 16, 2015, 2:42:39 AM3/16/15
to material...@googlegroups.com

Dear Expert,

 

Our vendor had purchased normalized plates from Sumitomo of steel making and Mill Cert clearly stated that the plates have been normalized but no sign or stamp “N” on plate. The problem is when the client reviewed and witnessed it, they don’t believe that the plate has been normalized and the question is what test needs to be conducted to prove that the plate has been normalized?

 

For your info: what do you think if the client ask for the following test:

1.       Tensile test and the specimen needs to be normalized first prior to test, acceptance criteria as per mill cert.

2.       Scanning Electron Microscope (SEM), acceptance criteria: no residual stress in the plate.

 

Your quick response is highly appreciated.

 

Regards

Dani

Gopalakrishnan G

unread,
Mar 16, 2015, 11:17:07 PM3/16/15
to material...@googlegroups.com
As per my point of view ,above stated 1&2 criteria acceptable then u can proceed.  

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.

For more options, visit https://groups.google.com/d/optout.



--
G.Gopalakrishnan
Welding Engineer
Mukand Ltd
Mumbai
Moble :+91-9833397917

Rems Okonkwo

unread,
Mar 16, 2015, 11:17:23 PM3/16/15
to material...@googlegroups.com
Hello Raj,
 
While Working on any project, you need to consider the client specification and the reference Code/Standard as stipulated in the contract document. Where there is conflit, the most strigent condition supercedes or issue a technical query to your client for clarification.
 
As per your query, you will need to check your client specification, they may have specifiy that PWHT is performed on such thinckness as 38mm and beside, your qualify WPS shall be limited to PWHT requirement and cannot be used otherwise.
 
I have a question for you, why did you qualify the WPS with PWHT if you do not want to use it and if you know the requirement of API 1104. What was on your mind when you are performing the WPQR and to what code have you qualified it?
 
Regards,
 
Rems Okonkwo (IWE)

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.

Nandesh Kumar

unread,
Mar 16, 2015, 11:17:37 PM3/16/15
to material...@googlegroups.com
Addition to my previous reply on the below query:
As per 13.1.2 of ASTM A20 (Plates for Pressure Vessels)
"Plates that are required to be heat treated, and have been so heat treated, shall be marked by the party that performed the heat treatment, with the letters “MT” (denoting material treated) following the required ASTM designation mark"


ವಂದನೆಗಳೊಂದಿಗೆ / Best regards,

Nandesh Kumar Arasappa

P.S. : Please don't print this e-mail unless you really need to.

--------------------------------------------
On Sat, 14/3/15, Dani Darwis <dan...@centrin.net.id> wrote:

Subject: [MW:22971] Normalized plate of A516 gr 70
To: material...@googlegroups.com
Date: Saturday, 14 March, 2015, 5:44 PM

#yiv9294488321
#yiv9294488321 --

_filtered #yiv9294488321 {panose-1:2 4 5 3 5 4 6 3 2 4;}
_filtered #yiv9294488321 {font-family:Calibri;panose-1:2 15
5 2 2 2 4 10 2 4;}
_filtered #yiv9294488321 {font-family:Tahoma;panose-1:2 11
6 4 3 5 4 4 2 4;}
#yiv9294488321
#yiv9294488321 p.yiv9294488321MsoNormal, #yiv9294488321
li.yiv9294488321MsoNormal, #yiv9294488321
div.yiv9294488321MsoNormal
{margin:0cm;margin-bottom:.0001pt;font-size:12.0pt;}
#yiv9294488321 a:link, #yiv9294488321
span.yiv9294488321MsoHyperlink
{color:blue;text-decoration:underline;}
#yiv9294488321 a:visited, #yiv9294488321
span.yiv9294488321MsoHyperlinkFollowed
{color:purple;text-decoration:underline;}
#yiv9294488321 p
{margin-right:0cm;margin-left:0cm;font-size:12.0pt;}
#yiv9294488321 p.yiv9294488321MsoAcetate, #yiv9294488321
li.yiv9294488321MsoAcetate, #yiv9294488321
div.yiv9294488321MsoAcetate
{margin:0cm;margin-bottom:.0001pt;font-size:8.0pt;}
#yiv9294488321 p.yiv9294488321MsoListParagraph,
#yiv9294488321 li.yiv9294488321MsoListParagraph,
#yiv9294488321 div.yiv9294488321MsoListParagraph
{margin-top:0cm;margin-right:0cm;margin-bottom:0cm;margin-left:36.0pt;margin-bottom:.0001pt;font-size:12.0pt;}
#yiv9294488321 span.yiv9294488321BalloonTextChar
{}
#yiv9294488321 span.yiv9294488321EmailStyle20
{color:#1F497D;}
#yiv9294488321 .yiv9294488321MsoChpDefault
{font-size:10.0pt;}
_filtered #yiv9294488321 {margin:72.0pt 72.0pt 72.0pt
72.0pt;}
#yiv9294488321 div.yiv9294488321WordSection1
{}
#yiv9294488321
_filtered #yiv9294488321 {}
_filtered #yiv9294488321 {}
_filtered #yiv9294488321 {}
_filtered #yiv9294488321 {}
#yiv9294488321 ol
{margin-bottom:0cm;}
#yiv9294488321 ul
{margin-bottom:0cm;}
#yiv9294488321 Dear Expert,  Our vendor had purchased
normalized plates from Sumitomo of steel making and Mill
Cert clearly stated that the plates have been normalized but
no sign or stamp “N” on plate. The problem is when the
client reviewed and witnessed it, they don’t believe that
the plate has been normalized and the question is what test
needs to be conducted to prove that the plate has been
normalized?  For your info: what do you think
if the client ask for the following test:1.       Tensile
test and the specimen needs to be normalized first prior to
test, acceptance criteria as per mill cert.2.       Scanning
Electron Microscope (SEM), acceptance criteria: no residual
stress in the plate.  Your quick response is highly
appreciated.  RegardsDani


--

You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails
from it, send an email to materials-weld...@googlegroups.com.

To post to this group, send email to material...@googlegroups.com.

Visit this group at http://groups.google.com/group/materials-welding.

To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/003101d05e5d%240d0168b0%2427043a10%24%40net.id.

Nandesh Kumar

unread,
Mar 16, 2015, 11:17:47 PM3/16/15
to material...@googlegroups.com
First of all, MTC shall state that the plate is Normalized. As long as the heat number on Plate is matching with the MTC, it as acceptable. There is no such rule that the N shall be stamped on the plate, unless it is for Hydrofluoric Service (to be stamped as 'HF-N'), as required by Supplementary requirements per S54.8 of ASTM A516.

ವಂದನೆಗಳೊಂದಿಗೆ / Best regards,

Nandesh Kumar Arasappa

P.S. : Please don't print this e-mail unless you really need to.

--------------------------------------------
On Sat, 14/3/15, Dani Darwis <dan...@centrin.net.id> wrote:

Subject: [MW:22971] Normalized plate of A516 gr 70
To: material...@googlegroups.com
Date: Saturday, 14 March, 2015, 5:44 PM

#yiv8143571543
#yiv8143571543 --

_filtered #yiv8143571543 {panose-1:2 4 5 3 5 4 6 3 2 4;}
_filtered #yiv8143571543 {font-family:Calibri;panose-1:2 15
5 2 2 2 4 10 2 4;}
_filtered #yiv8143571543 {font-family:Tahoma;panose-1:2 11
6 4 3 5 4 4 2 4;}
#yiv8143571543
#yiv8143571543 p.yiv8143571543MsoNormal, #yiv8143571543
li.yiv8143571543MsoNormal, #yiv8143571543
div.yiv8143571543MsoNormal
{margin:0cm;margin-bottom:.0001pt;font-size:12.0pt;}
#yiv8143571543 a:link, #yiv8143571543
span.yiv8143571543MsoHyperlink
{color:blue;text-decoration:underline;}
#yiv8143571543 a:visited, #yiv8143571543
span.yiv8143571543MsoHyperlinkFollowed
{color:purple;text-decoration:underline;}
#yiv8143571543 p
{margin-right:0cm;margin-left:0cm;font-size:12.0pt;}
#yiv8143571543 p.yiv8143571543MsoAcetate, #yiv8143571543
li.yiv8143571543MsoAcetate, #yiv8143571543
div.yiv8143571543MsoAcetate
{margin:0cm;margin-bottom:.0001pt;font-size:8.0pt;}
#yiv8143571543 p.yiv8143571543MsoListParagraph,
#yiv8143571543 li.yiv8143571543MsoListParagraph,
#yiv8143571543 div.yiv8143571543MsoListParagraph
{margin-top:0cm;margin-right:0cm;margin-bottom:0cm;margin-left:36.0pt;margin-bottom:.0001pt;font-size:12.0pt;}
#yiv8143571543 span.yiv8143571543BalloonTextChar
{}
#yiv8143571543 span.yiv8143571543EmailStyle20
{color:#1F497D;}
#yiv8143571543 .yiv8143571543MsoChpDefault
{font-size:10.0pt;}
_filtered #yiv8143571543 {margin:72.0pt 72.0pt 72.0pt
72.0pt;}
#yiv8143571543 div.yiv8143571543WordSection1
{}
#yiv8143571543
_filtered #yiv8143571543 {}
_filtered #yiv8143571543 {}
_filtered #yiv8143571543 {}
_filtered #yiv8143571543 {}
#yiv8143571543 ol
{margin-bottom:0cm;}
#yiv8143571543 ul
{margin-bottom:0cm;}
#yiv8143571543 Dear Expert,  Our vendor had purchased
normalized plates from Sumitomo of steel making and Mill
Cert clearly stated that the plates have been normalized but
no sign or stamp “N” on plate. The problem is when the
client reviewed and witnessed it, they don’t believe that
the plate has been normalized and the question is what test
needs to be conducted to prove that the plate has been
normalized?  For your info: what do you think
if the client ask for the following test:1.       Tensile
test and the specimen needs to be normalized first prior to
test, acceptance criteria as per mill cert.2.       Scanning
Electron Microscope (SEM), acceptance criteria: no residual
stress in the plate.  Your quick response is highly

meisam shokri arfaei

unread,
Mar 17, 2015, 11:51:22 PM3/17/15
to material...@googlegroups.com
Dear Dani,

For satisfaction of your client, you could do following:
1 - Metallography, But this test in this case may be risky, because of the effect of thermomechanical rolling and it is probable that you could not observe a big evidence.
2 - Impact testing, As the effect of normalizing process is to increase toughness, It could be more practical.

Regards


For more options, visit https://groups.google.com/d/optout.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer





Mhaskar Aly

unread,
Mar 19, 2015, 6:17:29 AM3/19/15
to material...@googlegroups.com
Dear Dani,
Write to mill and obtain letter of confirmation that heat treatment of plate done, also obtain authorization to stamp MT next Gr70 on plate, this may solve the purpose
Ali

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.

zhy3...@gmail.com

unread,
Sep 11, 2016, 2:55:41 AM9/11/16
to Materials & Welding

Dear raj:
    
    would you mind giving me a explanation about  whether PWHT is applied for following pipeline
    sour condensate pipeline  
    diameter : 20 inch  thickness: 10mm  length :164km
 




Alan Denney

unread,
Sep 11, 2016, 6:25:08 AM9/11/16
to material...@googlegroups.com

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---

You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.


For more options, visit https://groups.google.com/d/optout.


This email has been scanned by BullGuard antivirus protection.
For more info visit www.bullguard.com

zhy3...@gmail.com

unread,
Sep 14, 2016, 11:00:39 PM9/14/16
to Materials & Welding


在 2015年3月5日星期四 UTC+8下午6:36:41,Amul Raj写道:

Alan Denney

unread,
Sep 15, 2016, 5:58:13 AM9/15/16
to material...@googlegroups.com

 

Alan Denney

AKD Materials Consulting Ltd

 


Sent: 14 September 2016 16:03
To: Materials & Welding <material...@googlegroups.com>

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.


For more options, visit https://groups.google.com/d/optout.

Reply all
Reply to author
Forward
0 new messages