Dear Experts,

We need to qualify a PQR for S355 J2W Corten Steel Plates and I request you to suggest a suitable electrode and provide me a PWPS for S355 J2W.

Thanks in advance.

Sincerely,
Vijay 

srinivasu

unread,
Mar 4, 2015, 6:55:04 AM3/4/15
to material...@googlegroups.com

Suitable electrode for this combination is E8018-W2

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMBpsEd-ASMJ2QdVkyeb%2B8hCdJULufvc6O2uwB5X8d_RX33u-A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

c sridhar

unread,
Mar 6, 2015, 6:39:55 AM3/6/15
to material...@googlegroups.com
When welding Corten the precautions are similar to mild steel except that you may need
a special filler material to produce the weathering steel weld. (6013s are not acceptable.)
  • If the plate is 10mm thick or less, and the weld is a single pass (eg a fillet weld), 
    you can use an E7018 or SG2 MIG wire. This is because you will get enough dilution 
    from the plate to render the weld weathering.
  • If it's greater than 10mm thick or a multi-pass weld you need to use a filler containing 
    approximately 1% Nickel and 0.5% Copper (otherwise mild steel), or one containing 
    2.5% Nickel (otherwise mild steel).
This will result in a weld which will “weather” like the plate.
E 8018-C1, E 8018NiCuCr are also recommended for welding Corten steels.

Hence it is easy to make WPS

C Sridhar.
Technical Adviser - Welding,
for Alsta Pristine Engineering Private Limited,. Bangalore

( SS, AL fabricators & A venture of Advance Eng. Training & Inspection Services). Chennai,

Mobile nos: 0 94449 71097, 0 7406 326326, 0 94445 21267.


Please don't print this e-mail unless you really need to. Save the environment.




 


From: Vijay <k.vij...@gmail.com>
To: materials-welding <material...@googlegroups.com>
Sent: Wednesday, 4 March 2015 2:30 PM
Subject: [MW:22930] SUITABLE ELECTRODE FOR S355 J2W CORTEN STEEL

Reply all
Reply to author
Forward
0 new messages