RT/UT OF SOCKET WELD/BRANCH WELD

1,421 views
Skip to first unread message

Jignesh Desai

unread,
Nov 30, 2010, 11:52:07 AM11/30/10
to material...@googlegroups.com
Few days ago i came across UOP specification 8-11-12-Piping, which asked radiography of socket / branch welds for low alloy steel/SS. If somebody has done project with UOP in past, pl share their experience.


Also i read one very old B 31.3 Interpretation: 5-13 for the radiography of socket welds as below...

Subject:ANSI/ASME 831.3-1984 Edition, With the ANSI/ASME 831.3a-1984 Addenda, Table 327.4.1A, Limitations on Imperfections in Welds-Internal Porosity 
Date Issued: December 2, 1986

Question (1): In ANSI/ASME 831.3, Table 327.4.1 A, under internal porosity forfillet, socket, seal and reinforcement attachment welds, the wording NA (not applicable) is indicated. Does this mean that radiographic examination is not required for this type of joint configuration?

Reply (1): Yes.

In my opinion, RT of SW is only performed to detect the gap between two components, also in past during some corossion isometric study, we have assigned TML (thikness monitoring location) to carry out RT of SW/BW to confirm the correctness of welded heavy schedule components.

Can any one write few words about the technical feasibility and effectiveness of final result to confirm the soundness of SW/Branch weld by RT/UT with code back up? If somebody have any digital RT film of SW joint pl share.

Best Regds

paresh k patel

unread,
Dec 1, 2010, 1:47:39 AM12/1/10
to material...@googlegroups.com
Dear Jignesh

Hi! How are you? Hope fine.

Yes this is carried out to detect gap. In many companies this practice is adopted to verify gap for SW joints.

Regards

Paresh Patel
ABS IV


On Wed, 01 Dec 2010 07:17:32 +0530 wrote
--
>
To post to this group, send email to material...@googlegroups.com
>
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

Raghuram Bathula

unread,
Dec 1, 2010, 2:31:11 AM12/1/10
to Materials & Welding
Yes it is common to check 5% or 10% of welds, but 100% RT as specified
in this stnadard is something strange.

On Dec 1, 11:47 am, "paresh k patel" <pkpatel1...@rediffmail.com>
wrote:

Ahmed Husain

unread,
Dec 1, 2010, 9:46:45 AM12/1/10
to material...@googlegroups.com
It is also ARAMCO requirement  to take NDT to verify gaps in SW joints.

 

Regards,

AHusain
 



From: Raghuram Bathula <raghura...@gmail.com>
To: Materials & Welding <material...@googlegroups.com>
Sent: Wed, December 1, 2010 10:31:11 AM
Subject: [MW:8461] Re: RT/UT OF SOCKET WELD/BRANCH WELD
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

marcelo

unread,
Dec 6, 2010, 3:44:21 AM12/6/10
to Materials & Welding
dear all,

for my understanding of rt with socket welds especially in high temp
service is to ensure that the gap is there so the material is allowed
in termal expansions to avoid pushing the fillet weld during in
service condition.

thanks,
marcelo p soriano
qa/qc engineer

On Nov 30, 7:52 pm, Jignesh Desai <jignesh.desai....@gmail.com> wrote:
> Few days ago i came across *UOP specification 8-11-12-Piping*, which asked
> radiography of socket / branch welds for low alloy steel/SS. If somebody has
> done project with UOP in past, pl share their experience.
>
> *Also i read one very old B 31.3 Interpretation: 5-13 for the radiography of
> socket welds as below...*
> *
> *
> *Subject:ANSI/ASME 831.3-1984 Edition, With the ANSI/ASME 831.3a-1984
> Addenda, Table 327.4.1A, Limitations on Imperfections in Welds-Internal
> Porosity *
> *Date Issued: December 2, 1986*
> *
> *
> *Question (1): In ANSI/ASME 831.3, Table 327.4.1 A, under internal porosity
> forfillet, socket, seal and reinforcement attachment welds, the wording NA
> (not applicable) is indicated. Does this mean that radiographic examination
> is not required for this type of joint configuration?*
> *
> *
> *Reply (1): Yes.*