Are the but welding joint in annular plate of tank must be RT or not as per API 650?

Thanks

Samy

unread,
Sep 9, 2019, 12:06:07 AM9/9/19
to Materials & Welding
API Calls the below:

6.1.2.9 When bottom annular plates are required by 3.5.1, or by M.4.1, the radial joints shall be radiographed as
follows: (a) For double-welded butt joints, one spot radiograph shall be taken on 10% of the radial joints; (b) For single-welded butt joints with permanent or removable backup bar, one spot radiograph shall be taken on 50% of the radial joints. Extra carc must bc cxcrciscd in thc intcrprctation of radiographs of single-welded joints that have a permanent backup bar. In some cases, additional exposures taken at an angle may determine whether questionable indications are acceptable. The minimum radiographic length of each radial joint shall be 150 mm (6 in.). Locations of radiographs shall preferably be at the outer edge of the joint where the shell-plate and annular plate join. 

 - 3.5.1 clarifies the group classification
-  M4.1 Clarifies the tank dia.

Hope the above clarifies.

Sangram

unread,
Sep 9, 2019, 1:53:06 AM9/9/19
to material...@googlegroups.com
Dear Basem
Yes as per API-650 you need to be radiograph at least one spot on 50% of total joints.

Regards 
Sangramkeshari Routray 
Welding inspector 

Sent from my iPhone
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACct1WHdS23%2BJ-gP9DybDPqfOqqUKDssOugYqYAjrY%2B8zYrEgg%40mail.gmail.com.

basem elabd

unread,
Sep 9, 2019, 5:31:02 AM9/9/19
to material...@googlegroups.com
Dear, sangram

What the meaning of radial joint ?

Thanks for your cooperation 

Basel Salih

unread,
Sep 9, 2019, 7:04:15 AM9/9/19
to Materials & Welding
When you use Annular Plate around the bottom plate there are 2 type of joints 
1- Circumferential weld between Annular and Bottom plate.
2- Radial Weld between each of 2 Annular plates .



On Monday, September 9, 2019 at 12:31:02 PM UTC+3, basem elabd wrote:
Dear, sangram

What the meaning of radial joint ?

Thanks for your cooperation 

On Mon, Sep 9, 2019, 07:53 'Sangram' via Materials & Welding <material...@googlegroups.com> wrote:
Dear Basem
Yes as per API-650 you need to be radiograph at least one spot on 50% of total joints.

Regards 
Sangramkeshari Routray 
Welding inspector 

Sent from my iPhone

On 07-Sep-2019, at 12:08 AM, basem elabd <eng.ba...@gmail.com> wrote:

Dear all

Are the but welding joint in annular plate of tank must be RT or not as per API 650?

Thanks

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
annular plate.PNG

Sangram

unread,
Sep 9, 2019, 7:07:11 AM9/9/19
to material...@googlegroups.com
Dear Basem
If you have 14 joints in one tank you have take 7 spots in any 7 joints . 

Regards 
Sangramkeshari Routaray 
Welding inspector 

Sent from my iPhone