Dear Experts,

Can anyone suggest welding consumables for welding of SA 537 CL 2 ?

And precautions during welding.

Thanks,

Prakash Hegde

unread,
Jan 18, 2020, 11:37:33 PM1/18/20
to material...@googlegroups.com
Hi!
However what are the requirement?
Like
Impact test temp.Thk of weld n plate.Process being used . PWHT tem n time  consumables used
On this basis you can decide parameters and  precautions to be followed
Regards
Hegde
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CABDq6ghMxsVcLvE9XAqhUQutToi5dP8_-x30A6RdUcjKdpzSfg%40mail.gmail.com.

Revdiwala Darshan

unread,
Jan 20, 2020, 1:33:14 AM1/20/20
to material...@googlegroups.com
Dear Mr. Prakash,

Thanks for your reply, the details are mentioned below for your reference.

Impact required at MDMT -45
Service is Wet sour
There are different thicknesses from 20mm to 70mm.
PWHT Expected at 635 +/- 10 Deg.
PWHT Soaking Time max. 10 hours and Min. 1 hour.

Thanks & Regards,
Darshan

Prakash Gotimukul

unread,
Jan 20, 2020, 2:27:54 AM1/20/20
to materials-welding
Please do not refer replies by name. This is a group created with common interest. Question may be raised by anyone but the amswer is addressed to all member and is beneficial to all members.
When ever a reply is given either give references of code or say its your opinion based on your personal experience.

FOUNDER MEMBER
Thanks & Rgds.
Prakash Gotimukul
Authorised Inspection Supervisor
AIA LLC TX USA
MOB +97155 7114671
           +919730039755

Ahmed Osman

unread,
Jan 20, 2020, 3:25:37 AM1/20/20
to material...@googlegroups.com
Dears ,

1 - u can use 9018-D1 will give (20J @ -50C) CVN .. also after PWHT hardness will be around 200HV10 
2 - u can use 8018-C1 will give (20J @ -60C) CVN ... but Ni is not recommended in wet sour service 
so , you can go to 1st choice Mn-Mo elecreod

Best Regards ,
Ahmed Osman