Dear Expert,

During a site observation, a subcontractor's carbon steel shell (EH36, thickness 40 mm) was found re-rolled due to ovality after 100% of the NDT(UT&MPI) long seam welds. Many stresses come and grain boundaries are stretched after rolling such a thick joint.Any experts please advise.

Standard - DNV-OSC -401
Construction specifications - AWS D1.1
image.png


Thanks & Regards

Rajesh

Vishwas Keskar

unread,
Sep 27, 2023, 10:46:50 AM9/27/23
to material...@googlegroups.com, Rajesh Kumar
This is Carbon steel . Should not be any issue with L seam soundness.
Pl repeat NDT 
Thanks 
Vishwas  -IWE
9823472273

Sent from my iPhone

On 27-Sep-2023, at 7:22 PM, RAJESH KUMAR <rajeshkum...@gmail.com> wrote:


Dear Expert,

During a site observation, a subcontractor's carbon steel shell (EH36, thickness 40 mm) was found re-rolled due to ovality after 100% of the NDT(UT&MPI) long seam welds. Many stresses come and grain boundaries are stretched after rolling such a thick joint.Any experts please advise.

Standard - DNV-OSC -401
Construction specifications - AWS D1.1
<image.png>



Thanks & Regards

Rajesh

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMtcSfO5WESSOFt_GNicQH25ffSSuAHHGSSfNkCMp2FRCzLAMQ%40mail.gmail.com.

SENTHILKUMAR SWAMINATHAN

unread,
Sep 27, 2023, 10:46:50 AM9/27/23
to materials-welding, Rajesh Kumar
Re-do All NDT Performed before rolling. Volumetric NDT Results should compare with before rolling. (Ex. Radiographs before and after compare it)  

Thank you, 
Regards, 
S.SENTHILKUMAR


Dhaneesh p

unread,
Sep 28, 2023, 1:05:46 AM9/28/23
to material...@googlegroups.com
Hi 

No issues .. kindly proceed rerolling and after that do volumetric and surface NDT 

Regards 
Dhaneesh 

james gerald

unread,
Sep 28, 2023, 1:05:46 AM9/28/23
to material...@googlegroups.com
I suppose this is a structural material. Rerolling does not reduce the Material Thickness and it is done to obtain uniform curvature and does not induce any stresses. In structural material, even Flame straightening below 600 deg C is permitted.