PWHT criteria for NACE material

273 views
Skip to first unread message

pradip kumar sil

unread,
Sep 14, 2011, 3:22:13 AM9/14/11
to material...@googlegroups.com
Dear Exparts,
Can anybody tell me, NACE carbon steel PWHT heating/ cooling rate
where is it mentioned.
Regards
Pradip

manivannan hemu

unread,
Sep 14, 2011, 5:14:29 AM9/14/11
to material...@googlegroups.com
Hi Pradip,

to my understanding NACE RP 0472 has guidelines for controlling
cracking by adopting the use of PWHT for Carbon steel weldments. This
recommended practice did specify the PWHT, heating rate and cooling
rate to be followed asper ASME construction code. (refer para 6.4 of
the above).

NACE RP is attached for your understanding.

Regards,
Manivannan.
Manger QA
Flowlink systems.Coimbatore.

> --
> To post to this group, send email to material...@googlegroups.com
> To unsubscribe from this group, send email to
> materials-weld...@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>


--
*Manivannan.p*

NACE RP 0472.pdf

Eswaran samikannu

unread,
Sep 14, 2011, 6:16:50 AM9/14/11
to material...@googlegroups.com
Hi Pradip,
 
Heating above 300 Deg C - APP Max 150 Deg C / Hr up to Soaking temperature around 620 Deg C ,It should below Tempering temperature of your product
 
Cooling rate - APP Max 150 Deg C / Hr up to 300 Deg C temperature after you can cool in air, you can get HRC Value below 22.
Refer the stress relieving temp at A.2.14 Welding in NACE book
By 
Jegan  

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

Raghuram Bathula

unread,
Sep 14, 2011, 7:18:34 AM9/14/11
to material...@googlegroups.com
please donot ditrubute codes/standards neither ask for it